Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.24 g/cm³ Show Supplier Material materials with Dichte of 1.24 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.11 % Show Supplier Material materials with Moisture absorption of 0.11 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 0.27 % Show Supplier Material materials with Wasserabsorption of 0.27 % | dry | ISO 62 | at 23°C after 24h |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | dry | ISO 527-1/-2 | ||
Elastizitätsmodul | 0.16 GPa Show Supplier Material materials with Elastizitätsmodul of 0.16 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 38 % Show Supplier Material materials with Elongation at yield of 38 % | dry | ISO 527-1/-2 | ||
Härte, Shore A | 98 [-] Show Supplier Material materials with Härte, Shore A of 98 [-] | dry | ISO 868 | 3s | |
98 [-] Show Supplier Material materials with Härte, Shore A of 98 [-] | dry | ISO 868 | 15s | ||
Härte, Shore D | 51 [-] Show Supplier Material materials with Härte, Shore D of 51 [-] | dry | ISO 868 | 3s | |
51 [-] Show Supplier Material materials with Härte, Shore D of 51 [-] | dry | ISO 868 | 15s | ||
Reißfestigkeit | 146 kN/m Show Supplier Material materials with Reißfestigkeit of 146 kN/m | dry | ISO 34-1; Method B | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 5.6 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5.6 kJ/m² | dry | ISO 179/1eA | |
Zugfestigkeit | 32 MPa Show Supplier Material materials with Zugfestigkeit of 32 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Glasübergangstemperatur | -10 °C Show Supplier Material materials with Glasübergangstemperatur of -10 °C | dry | ISO 11357-1/-2 | 10°C/min |
Schmelzpunkt | 205 °C Show Supplier Material materials with Schmelzpunkt of 205 °C | dry | ISO 11357-1/-3 | 10°C/min |
Vicat-Erweichungstemperatur | 61 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 61 °C | dry | ISO 306 | 50°C/h 50N |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.58 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.58 [-] | dry | IEC 62631-2-1 | 1MHz |
4.34 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.34 [-] | dry | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 15 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 15 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 212 [-] Show Supplier Material materials with Verlustfaktor of 212 [-] | dry | IEC 62631-2-1 | 100Hz |
460 [-] Show Supplier Material materials with Verlustfaktor of 460 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 8 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 8 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|