Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.55 g/cm³ Show Supplier Material materials with Dichte of 1.55 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.05 % Show Supplier Material materials with Moisture absorption of 0.05 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 0.05 % Show Supplier Material materials with Wasserabsorption of 0.05 % | dry | ISO 62 | at 23°C after 24h |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 10 GPa Show Supplier Material materials with Biegemodul of 10 GPa | dry | ISO 178 | |
120 °C | 4.5 GPa Show Supplier Material materials with Biegemodul of 4.5 GPa | dry | ISO 178 | |
160 °C | 3.3 GPa Show Supplier Material materials with Biegemodul of 3.3 GPa | dry | ISO 178 | |
200 °C | 2.9 GPa Show Supplier Material materials with Biegemodul of 2.9 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 | ||
120 °C | 4.6 % Show Supplier Material materials with Dehnung of 4.6 % | dry | ISO 527-1/-2 | |
160 °C | 5.3 % Show Supplier Material materials with Dehnung of 5.3 % | dry | ISO 527-1/-2 | |
200 °C | 5.4 % Show Supplier Material materials with Dehnung of 5.4 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 12 GPa Show Supplier Material materials with Elastizitätsmodul of 12 GPa | dry | ISO 527-1/-2 |
12 GPa Show Supplier Material materials with Elastizitätsmodul of 12 GPa | dry | ISO 527-1/-2 | ||
120 °C | 4.7 GPa Show Supplier Material materials with Elastizitätsmodul of 4.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.5 GPa Show Supplier Material materials with Elastizitätsmodul of 3.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.0 GPa Show Supplier Material materials with Elastizitätsmodul of 3.0 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 240 MPa Show Supplier Material materials with Flexural yield strength of 240 MPa | dry | ISO 178 | |
120 °C | 96 MPa Show Supplier Material materials with Flexural yield strength of 96 MPa | dry | ISO 178 | |
160 °C | 68 MPa Show Supplier Material materials with Flexural yield strength of 68 MPa | dry | ISO 178 | |
200 °C | 56.0 MPa Show Supplier Material materials with Flexural yield strength of 56.0 MPa | dry | ISO 178 | |
Hardness, Rockwell R | 120 [-] Show Supplier Material materials with Hardness, Rockwell R of 120 [-] | dry | ISO 2039-2 | |
Härte, Rockwell M | 100 [-] Show Supplier Material materials with Härte, Rockwell M of 100 [-] | dry | ISO 2039-2 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | dry | ISO 179/1eA |
23 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 56.0 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 56.0 kJ/m² | dry | ISO 179/1eU |
23 °C | 58.0 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 58.0 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 185 MPa Show Supplier Material materials with Zugfestigkeit of 185 MPa | dry | ISO 527-1/-2 |
170 MPa Show Supplier Material materials with Zugfestigkeit of 170 MPa | dry | ISO 527-1/-2 | ||
120 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 | |
160 °C | 55.0 MPa Show Supplier Material materials with Zugfestigkeit of 55.0 MPa | dry | ISO 527-1/-2 | |
200 °C | 45 MPa Show Supplier Material materials with Zugfestigkeit of 45 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Glasübergangstemperatur | 90 °C Show Supplier Material materials with Glasübergangstemperatur of 90 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Koeffizient der thermischen Ausdehnung | 1.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | |||
5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
1.2e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.2e-06 1/K | dry | ISO 11359-1/-2 | normal, above Tg | |||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.4 mm | ||
Schmelzpunkt | 280 °C Show Supplier Material materials with Schmelzpunkt of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 185 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 185 °C | dry | ISO 75-1/-2 | 8 MPa | ||
265 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 265 °C | dry | ISO 75-1/-2 | 2 MPa | |||
280 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 280 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.8 [-] | dry | IEC 60250 | 1GHz |
3.8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.8 [-] | dry | IEC 60250 | 5GHz | |
Durchschlagfestigkeit | 34 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 34 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 175 V Show Supplier Material materials with Kriechstromfestigkeit of 175 V | dry | IEC 60112 | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | |
Verlustfaktor | 30 [-] Show Supplier Material materials with Verlustfaktor of 30 [-] | dry | IEC 60250 | 1GHz |
45 [-] Show Supplier Material materials with Verlustfaktor of 45 [-] | dry | IEC 60250 | 5GHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | ADAS Radar Housing | |
Fillers | 30% Glass Fiber |