Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.35 g/cm³ Show Supplier Material materials with Dichte of 1.35 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.9 % Show Supplier Material materials with Moisture absorption of 1.9 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.3 % Show Supplier Material materials with Wasserabsorption of 6.3 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
12 % Show Supplier Material materials with Dehnung of 12 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 3 GPa Show Supplier Material materials with Elastizitätsmodul of 3 GPa | conditioned | ISO 527-1/-2 | |
6.2 GPa Show Supplier Material materials with Elastizitätsmodul of 6.2 GPa | dry | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | dry | ISO 179/1eA | |
23 °C | 7 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 30 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 30 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 35 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 35 kJ/m² | dry | ISO 179/1eU | |
23 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | conditioned | ISO 527-1/-2 | |
115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | HB | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Koeffizient der thermischen Ausdehnung | 3.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | 0.75 mm | UL746B | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperaturleitfähigkeit | 1.43e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.43e-07 mm²/s | dry | - | |||
Wärmeformbeständigkeitstemperatur | 195 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 195 °C | dry | ISO 75-1/-2 | 2 MPa | ||
215 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | conditioned | IEC 60243-1 | |
35 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 35 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 350 V Show Supplier Material materials with Kriechstromfestigkeit of 350 V | conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 50 [-] Show Supplier Material materials with Verlustfaktor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Verlustfaktor of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Verlustfaktor of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 1190 g/cm³ Show Supplier Material materials with Density of melt of 1190 g/cm³ | dry | - | ||
Schmelzmassenflussrate | 275 °C | 72 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 72 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 250 °C | 10 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 10 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 0.7 % Show Supplier Material materials with Schrumpfung of 0.7 % | dry | ISO 294-4 | Parallel | |
1.2 % Show Supplier Material materials with Schrumpfung of 1.2 % | dry | ISO 294-4 | Normal | ||
Specific heat capacity melt | 2230 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2230 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.29 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.29 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber and Glass Bead |