Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.58 g/cm³ Show Supplier Material materials with Dichte of 1.58 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 1.8 % Show Supplier Material materials with Wasserabsorption of 1.8 % | dry | ISO 62 | at 23°C after 24h |
4.8 % Show Supplier Material materials with Wasserabsorption of 4.8 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 16 GPa Show Supplier Material materials with Biegemodul of 16 GPa | dry | ISO 178 | |
120 °C | 7.3 GPa Show Supplier Material materials with Biegemodul of 7.3 GPa | dry | ISO 178 | |
160 °C | 6.5 GPa Show Supplier Material materials with Biegemodul of 6.5 GPa | dry | ISO 178 | |
180 °C | 5.8 GPa Show Supplier Material materials with Biegemodul of 5.8 GPa | dry | ISO 178 | |
200 °C | 5.2 GPa Show Supplier Material materials with Biegemodul of 5.2 GPa | dry | ISO 178 | |
210 °C | 4.9 GPa Show Supplier Material materials with Biegemodul of 4.9 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2.6 % Show Supplier Material materials with Dehnung of 2.6 % | dry | ISO 527-1/-2 |
2.8 % Show Supplier Material materials with Dehnung of 2.8 % | dry | ISO 527-1/-2 | ||
4.6 % Show Supplier Material materials with Dehnung of 4.6 % | conditioned | ISO 527-1/-2 | ||
120 °C | 6.7 % Show Supplier Material materials with Dehnung of 6.7 % | dry | ISO 527-1/-2 | |
150 °C | 6.9 % Show Supplier Material materials with Dehnung of 6.9 % | dry | ISO 527-1/-2 | |
160 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
180 °C | 7.1 % Show Supplier Material materials with Dehnung of 7.1 % | dry | ISO 527-1/-2 | |
200 °C | 7.2 % Show Supplier Material materials with Dehnung of 7.2 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 17 GPa Show Supplier Material materials with Elastizitätsmodul of 17 GPa | dry | ISO 527-1/-2 |
10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | conditioned | ISO 527-1/-2 | ||
16.5 GPa Show Supplier Material materials with Elastizitätsmodul of 16.5 GPa | dry | ISO 527-1/-2 | ||
40 °C | 15 GPa Show Supplier Material materials with Elastizitätsmodul of 15 GPa | dry | ISO 527-1/-2 | |
100 °C | 7.1 GPa Show Supplier Material materials with Elastizitätsmodul of 7.1 GPa | dry | ISO 527-1/-2 | |
120 °C | 6.7 GPa Show Supplier Material materials with Elastizitätsmodul of 6.7 GPa | dry | ISO 527-1/-2 | |
150 °C | 5.6 GPa Show Supplier Material materials with Elastizitätsmodul of 5.6 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.7 GPa Show Supplier Material materials with Elastizitätsmodul of 4.7 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.1 GPa Show Supplier Material materials with Elastizitätsmodul of 4.1 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 360 MPa Show Supplier Material materials with Flexural yield strength of 360 MPa | dry | ISO 178 | |
120 °C | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | dry | ISO 178 | |
160 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
180 °C | 108 MPa Show Supplier Material materials with Flexural yield strength of 108 MPa | dry | ISO 178 | |
200 °C | 87 MPa Show Supplier Material materials with Flexural yield strength of 87 MPa | dry | ISO 178 | |
210 °C | 80 MPa Show Supplier Material materials with Flexural yield strength of 80 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 14.0 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 14.0 kJ/m² | dry | ISO 179/1eA |
-30 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 15.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 15.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 25 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 25 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | dry | ISO 179/1eU |
-30 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 95 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 95 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 100 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 300 MPa Show Supplier Material materials with Zugfestigkeit of 300 MPa | dry | ISO 527-1/-2 |
145 MPa Show Supplier Material materials with Zugfestigkeit of 145 MPa | conditioned | ISO 527-1/-2 | ||
235 MPa Show Supplier Material materials with Zugfestigkeit of 235 MPa | dry | ISO 527-1/-2 | ||
100 °C | 120 MPa Show Supplier Material materials with Zugfestigkeit of 120 MPa | dry | ISO 527-1/-2 | |
120 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | dry | ISO 527-1/-2 | |
150 °C | 90 MPa Show Supplier Material materials with Zugfestigkeit of 90 MPa | dry | ISO 527-1/-2 | |
160 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
180 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 | |
200 °C | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Schmelzpunkt | 260 °C Show Supplier Material materials with Schmelzpunkt of 260 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 245 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 245 °C | dry | ISO 75-1/-2 | 2 MPa | |
255 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 255 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Integrated Air Inlet Manifolds (up to 180°C), Resonators and ByPass Valves, Charge Air Cooler Caps | |
Fillers | 50% Glass Fiber |