Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.4 g/cm³ Show Supplier Material materials with Dichte of 1.4 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.18 % Show Supplier Material materials with Moisture absorption of 0.18 % | dry | Sim. to ISO 62 |
Wasserabsorption | 0.45 % Show Supplier Material materials with Wasserabsorption of 0.45 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.4 GPa Show Supplier Material materials with Biegemodul of 2.4 GPa | dry | ISO 178 | |
120 °C | 0.38 GPa Show Supplier Material materials with Biegemodul of 0.38 GPa | dry | ISO 178 | |
160 °C | 0.16 GPa Show Supplier Material materials with Biegemodul of 0.16 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 10 % Show Supplier Material materials with Dehnung of 10 % | dry | ISO 527-1/-2 |
13 % Show Supplier Material materials with Dehnung of 13 % | dry | ISO 527-1/-2 | ||
120 °C | 130 % Show Supplier Material materials with Dehnung of 130 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 3.4 GPa Show Supplier Material materials with Elastizitätsmodul of 3.4 GPa | dry | ISO 527-1/-2 |
2.6 GPa Show Supplier Material materials with Elastizitätsmodul of 2.6 GPa | dry | ISO 527-1/-2 | ||
100 °C | 0.45 GPa Show Supplier Material materials with Elastizitätsmodul of 0.45 GPa | dry | ISO 527-1/-2 | |
120 °C | 0.35 GPa Show Supplier Material materials with Elastizitätsmodul of 0.35 GPa | dry | ISO 527-1/-2 | |
160 °C | 0.15 GPa Show Supplier Material materials with Elastizitätsmodul of 0.15 GPa | dry | ISO 527-1/-2 | |
180 °C | 0.15 GPa Show Supplier Material materials with Elastizitätsmodul of 0.15 GPa | dry | ISO 527-1/-2 | |
Elongation at yield | -40 °C | 7 % Show Supplier Material materials with Elongation at yield of 7 % | dry | ISO 527-1/-2 |
4.5 % Show Supplier Material materials with Elongation at yield of 4.5 % | dry | ISO 527-1/-2 | ||
Flexural yield strength | 75 MPa Show Supplier Material materials with Flexural yield strength of 75 MPa | dry | ISO 178 | |
120 °C | 17 MPa Show Supplier Material materials with Flexural yield strength of 17 MPa | dry | ISO 178 | |
160 °C | 8 MPa Show Supplier Material materials with Flexural yield strength of 8 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 6 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6 kJ/m² | dry | ISO 179/1eA |
23 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 150 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 150 kJ/m² | dry | ISO 179/1eU |
Streckgrenze | -40 °C | 90 MPa Show Supplier Material materials with Streckgrenze of 90 MPa | dry | ISO 527-1/-2 |
50 MPa Show Supplier Material materials with Streckgrenze of 50 MPa | dry | ISO 527-1/-2 | ||
Zugfestigkeit | -40 °C | 90 MPa Show Supplier Material materials with Zugfestigkeit of 90 MPa | dry | ISO 527-1/-2 |
45 MPa Show Supplier Material materials with Zugfestigkeit of 45 MPa | dry | ISO 527-1/-2 | ||
100 °C | 25 MPa Show Supplier Material materials with Zugfestigkeit of 25 MPa | dry | ISO 527-1/-2 | |
120 °C | 20 MPa Show Supplier Material materials with Zugfestigkeit of 20 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | V-0 | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 2 mm | IEC 60695-2-12 | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 0.75 mm | IEC 60695-2-12 | |||
Glow Wire Ignition Temperature | 675 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 675 °C | dry | 2 mm | IEC 60695-2-13 | ||
900 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 900 °C | dry | 0.75 mm | IEC 60695-2-13 | |||
Koeffizient der thermischen Ausdehnung | 9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical impact | 110 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 110 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | 0.75 mm | UL746B | ||
Schmelzpunkt | 225 °C Show Supplier Material materials with Schmelzpunkt of 225 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 60 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 60 °C | dry | ISO 75-1/-2 | 2 MPa | ||
140 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 140 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.2 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.2 [-] | dry | IEC 62631-2-1 | 1MHz |
3.4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.4 [-] | dry | IEC 62631-2-1 | 100Hz | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 30 [-] Show Supplier Material materials with Verlustfaktor of 30 [-] | dry | IEC 62631-2-1 | 100Hz |
220 [-] Show Supplier Material materials with Verlustfaktor of 220 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzmassenflussrate | 250 °C | 4 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 4 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 250 °C | 5 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 5 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 2 % Show Supplier Material materials with Schrumpfung of 2 % | dry | ISO 294-4 | Normal | |
2.3 % Show Supplier Material materials with Schrumpfung of 2.3 % | dry | ISO 294-4 | Parallel |
Technological properties
Property | ||
---|---|---|
Application areas | White Good Connectors | |
Certifications | Yellow Card Available |