Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.67 g/cm³ Show Supplier Material materials with Dichte of 1.67 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 17 GPa Show Supplier Material materials with Biegemodul of 17 GPa | dry | ISO 178 | |
18 GPa Show Supplier Material materials with Biegemodul of 18 GPa | conditioned | ISO 178 | ||
Dehnung | 2 % Show Supplier Material materials with Dehnung of 2 % | conditioned | ISO 527-1/-2 | |
2.3 % Show Supplier Material materials with Dehnung of 2.3 % | dry | ISO 527-1/-2 | ||
Elastizitätsmodul | 18.5 GPa Show Supplier Material materials with Elastizitätsmodul of 18.5 GPa | dry | ISO 527-1/-2 | |
19 GPa Show Supplier Material materials with Elastizitätsmodul of 19 GPa | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 310 MPa Show Supplier Material materials with Flexural yield strength of 310 MPa | conditioned | ISO 178 | |
350 MPa Show Supplier Material materials with Flexural yield strength of 350 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | 23 °C | 12 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | conditioned | ISO 179/1eA |
23 °C | 13.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 13.5 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | conditioned | ISO 179/1eU |
23 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | 210 MPa Show Supplier Material materials with Zugfestigkeit of 210 MPa | conditioned | ISO 527-1/-2 | |
230 MPa Show Supplier Material materials with Zugfestigkeit of 230 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 120 °C Show Supplier Material materials with Glasübergangstemperatur of 120 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 1.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
4.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 315 °C Show Supplier Material materials with Schmelzpunkt of 315 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 250 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 250 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Durchschlagfestigkeit | 30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | dry | IEC 60243-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schrumpfung | 0.38 % Show Supplier Material materials with Schrumpfung of 0.38 % | dry | ISO 294-4 | Parallel |
0.59 % Show Supplier Material materials with Schrumpfung of 0.59 % | dry | ISO 294-4 | Normal | |
Spiral flow length | 60 | dry | - | 1.0 mm 800 bar |
75 | dry | - | 1.0 mm 1000 bar | |
90 | dry | - | 1.0 mm 1200 bar |
Technological properties
Property | ||
---|---|---|
Application areas | Notebook Housings, Medium Voltage Circuit Breakers, Medium Voltage Circuit Breakers Embedded Pole | |
Certifications | Yellow Card Available | |
Fillers | Glass Fiber |