Property | Value |
---|---|
Relative Dichte | 8.86 [-] Show Supplier Material materials with Relative Dichte of 8.86 [-] |
Mechanisch
Property | Value | Comment |
---|---|---|
Biegemodul | 110 GPa Show Supplier Material materials with Biegemodul of 110 GPa | |
Dehnung | 4 % Show Supplier Material materials with Dehnung of 4 % | min. | EH Temper | for thickness 0.2-5 mm |
7 % Show Supplier Material materials with Dehnung of 7 % | min. | H Temper | for thickness 0.1-5 mm | |
15 % Show Supplier Material materials with Dehnung of 15 % | min. | 1/2H Temper | for thickness 0.1-5 mm | |
28 % Show Supplier Material materials with Dehnung of 28 % | min. | 1/4H Temper | for thickness 0.1-5 mm | |
40 % Show Supplier Material materials with Dehnung of 40 % | min. | O Temper | for thickness 0.1-5 mm | |
Elastizitätsmodul | 115 GPa Show Supplier Material materials with Elastizitätsmodul of 115 GPa | |
Härte, Vickers | 90 - 160 [-] Show Supplier Material materials with Härte, Vickers of 90 - 160 [-] | 1/4H Temper | for thickness 0.1-5 mm |
130 - 190 [-] Show Supplier Material materials with Härte, Vickers of 130 - 190 [-] | 1/2H Temper | for thickness 0.1-5 mm | |
170 - 220 [-] Show Supplier Material materials with Härte, Vickers of 170 - 220 [-] | H Temper | for thickness 0.1-5 mm | |
190 - 230 [-] Show Supplier Material materials with Härte, Vickers of 190 - 230 [-] | EH Temper | for thickness 0.05-5 mm | |
200 [-] Show Supplier Material materials with Härte, Vickers of 200 [-] | min. | SH Temper | for thickness 0.05-5 mm | |
Zugfestigkeit | 305 MPa Show Supplier Material materials with Zugfestigkeit of 305 MPa | min. | O Temper | for thickness 0.1-5 mm |
375 - 470 MPa Show Supplier Material materials with Zugfestigkeit of 375 - 470 MPa | 1/4H Temper | for thickness 0.1-5 mm | |
470 - 570 MPa Show Supplier Material materials with Zugfestigkeit of 470 - 570 MPa | 1/2H Temper | for thickness 0.1-5 mm | |
570 - 665 MPa Show Supplier Material materials with Zugfestigkeit of 570 - 665 MPa | H Temper | for thickness 0.1-5 mm | |
620 - 710 MPa Show Supplier Material materials with Zugfestigkeit of 620 - 710 MPa | EH Temper | for thickness 0.1-5 mm | |
660 MPa Show Supplier Material materials with Zugfestigkeit of 660 MPa | min. | SH Temper | for thickness 0.1-5 mm |
Thermisch
Property | Value |
---|---|
Koeffizient der thermischen Ausdehnung | 1.78e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.78e-05 1/K |
Schmelzpunkt | 950 - 1050 °C Show Supplier Material materials with Schmelzpunkt of 950 - 1050 °C |
Spezifische Wärmekapazität | 377 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) |
Wärmeleitfähigkeit | 71 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 71 W/(m·K) |
Elektrisch
Property | Value |
---|---|
Specific Electrical conductivity | 17 % IACS Show Supplier Material materials with Specific Electrical conductivity of 17 % IACS |
Chemical properties
Property | Value | Comment |
---|---|---|
Andere | 99.5 % Show Supplier Material materials with Andere of 99.5 % | min. | Cu+Sn+P |
Blei | 0.02 % Show Supplier Material materials with Blei of 0.02 % | max. |
Eisen | 0.1 % Show Supplier Material materials with Eisen of 0.1 % | max. |
Phosphor | 0.03 - 0.35 % Show Supplier Material materials with Phosphor of 0.03 - 0.35 % | |
Zink | 0.2 % Show Supplier Material materials with Zink of 0.2 % | max. |
Zinn | 4.5 - 5.5 % Show Supplier Material materials with Zinn of 4.5 - 5.5 % |
Technological properties
Property | ||
---|---|---|
Application areas | The grade is particularly suitable for electronics (connectors, lead frames, lead terminals, transistor terminals, etc.), electrical (relay and switch contacts, rotary switch slides and contacts, fuse clips, etc.), automotive (bearing frames, hydraulic equipment caps, packing, bearings, clutch disks, electrical parts, etc.) and others (bellows, slides, blades, plate springs, corrosion-proof machinery equipment, diaphragms, etc.) | |
Coating | Standard product specification of a HOT-DIP-tinned strip. *Width means the slit width after plating. *Different plating thickness for each side is possible. * We can accommodate our products to individual specifications other than the above standard specifications. Please feel free to call us. | |
Other | Hardness Vickers note: Minimum test force is 1.961 N | |
Tolerances |