Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 12.7 % Show Material materials with Dehnung of 12.7 % | Predicted Value, A80 | ||||
12.7 % Show Material materials with Dehnung of 12.7 % | Predicted Value, A200 | |||||
15.9 % Show Material materials with Dehnung of 15.9 % | Predicted Value, Transverse | |||||
18.2 % Show Material materials with Dehnung of 18.2 % | Predicted Value, A5 | |||||
18.3 % Show Material materials with Dehnung of 18.3 % | Predicted Value, A80 Transverse | |||||
19.4 % Show Material materials with Dehnung of 19.4 % | Predicted Value, A50 | |||||
20 °C | 15 % Show Material materials with Dehnung of 15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
Elastizitätsmodul | 20 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
Flächenreduzierung | 40.3 % Show Material materials with Flächenreduzierung of 40.3 % | Predicted Value | ||||
44.8 % Show Material materials with Flächenreduzierung of 44.8 % | Predicted Value, Transverse | |||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Scherfestigkeit | 598.9 MPa Show Material materials with Scherfestigkeit of 598.9 MPa | Predicted Value | ||||
Schubmodule | 79.6 GPa Show Material materials with Schubmodule of 79.6 GPa | Predicted Value | ||||
Streckgrenze | 309.5 MPa Show Material materials with Streckgrenze of 309.5 MPa | Predicted Value, RP1 | ||||
329.7 MPa Show Material materials with Streckgrenze of 329.7 MPa | Predicted Value, RP1 Transverse | |||||
501.5 MPa Show Material materials with Streckgrenze of 501.5 MPa | Predicted Value, RP02 Transverse | |||||
528 MPa Show Material materials with Streckgrenze of 528 MPa | Predicted Value, Transverse | |||||
541.7 MPa Show Material materials with Streckgrenze of 541.7 MPa | Predicted Value, RP05 | |||||
570.1 MPa Show Material materials with Streckgrenze of 570.1 MPa | Predicted Value, RP02 | |||||
629.5 MPa Show Material materials with Streckgrenze of 629.5 MPa | Predicted Value, RP002 | |||||
20 °C | 560 MPa Show Material materials with Streckgrenze of 560 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 580 MPa Show Material materials with Streckgrenze of 580 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 620 MPa Show Material materials with Streckgrenze of 620 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
Zugfestigkeit | 20 °C | 650 - 890 MPa Show Material materials with Zugfestigkeit of 650 - 890 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | |
20 °C | 650 - 830 MPa Show Material materials with Zugfestigkeit of 650 - 830 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 700 - 890 MPa Show Material materials with Zugfestigkeit of 700 - 890 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 700 - 830 MPa Show Material materials with Zugfestigkeit of 700 - 830 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100 °C | 1.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Spezifische Wärmekapazität | 20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Wärmeleitfähigkeit | 20 °C | 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 5 S/m Show Material materials with Elektrische Leitfähigkeit of 5 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.7e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bor | 0.005 % Show Material materials with Bor of 0.005 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Chrom | 1.5 % Show Material materials with Chrom of 1.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Kupfer | 0.5 % Show Material materials with Kupfer of 0.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Mangan | 1.7 % Show Material materials with Mangan of 1.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Molybdän | 0.7 % Show Material materials with Molybdän of 0.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Nickel | 2 % Show Material materials with Nickel of 2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Niobium | 0.06 % Show Material materials with Niobium of 0.06 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Silizium | 0.8 % Show Material materials with Silizium of 0.8 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Stickstoff | 0.015 % Show Material materials with Stickstoff of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Vanadium | 0.12 % Show Material materials with Vanadium of 0.12 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Zirkonium | 0.15 % Show Material materials with Zirkonium of 0.15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |