Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 20.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Manganese Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A80, transversal | 20.0 °C | 26 % Show Material materials with Dehnung A80, transversal of 26 % | |
Elastizitätsmodul | 20.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Manganese Steel |
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Manganese Steel |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 300 - 360 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 300 - 360 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 400 - 480 MPa Show Material materials with Zugfestigkeit, transversal of 400 - 480 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.33E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.33E-5 1/K | Typical for Manganese Steel |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Manganese Steel | |
Spezifische Wärmekapazität | 20.0 °C | 510 - 553 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 510 - 553 J/(kg·K) | Typical for Manganese Steel |
Wärmeleitfähigkeit | 20.0 °C | 14 - 16 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14 - 16 W/(m·K) | Typical for Manganese Steel |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % |
Kohlenstoff | 0.11 % Show Material materials with Kohlenstoff of 0.11 % |
Mangan | 0.7 - 0.8 % Show Material materials with Mangan of 0.7 - 0.8 % |
Niobium | 0.09 % Show Material materials with Niobium of 0.09 % |
Phosphor | 0.12 % Show Material materials with Phosphor of 0.12 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % |
Titan | 0.12 % Show Material materials with Titan of 0.12 % |