Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.9 g/cm³ Show Material materials with Dichte of 7.9 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung, transversal | 20.0 °C | 35 % Show Material materials with Dehnung, transversal of 35 % | |
Elastizitätsmodul | 20.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Elastizitätsmodul of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 100.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 0,2 of 145 MPa | |
150.0 °C | 130 MPa Show Material materials with Streckgrenze Rp 0,2 of 130 MPa | ||
200.0 °C | 118 MPa Show Material materials with Streckgrenze Rp 0,2 of 118 MPa | ||
250.0 °C | 108 MPa Show Material materials with Streckgrenze Rp 0,2 of 108 MPa | ||
300.0 °C | 100 MPa Show Material materials with Streckgrenze Rp 0,2 of 100 MPa | ||
350.0 °C | 94 MPa Show Material materials with Streckgrenze Rp 0,2 of 94 MPa | ||
400.0 °C | 89 MPa Show Material materials with Streckgrenze Rp 0,2 of 89 MPa | ||
450.0 °C | 85 MPa Show Material materials with Streckgrenze Rp 0,2 of 85 MPa | ||
500.0 °C | 81 MPa Show Material materials with Streckgrenze Rp 0,2 of 81 MPa | ||
550.0 °C | 80 MPa Show Material materials with Streckgrenze Rp 0,2 of 80 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 175 MPa | |
Streckgrenze Rp 1,0 | 100.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 1,0 of 180 MPa | |
150.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 1,0 of 160 MPa | ||
200.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 1,0 of 145 MPa | ||
250.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 1,0 of 135 MPa | ||
300.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 1,0 of 127 MPa | ||
350.0 °C | 121 MPa Show Material materials with Streckgrenze Rp 1,0 of 121 MPa | ||
400.0 °C | 116 MPa Show Material materials with Streckgrenze Rp 1,0 of 116 MPa | ||
450.0 °C | 112 MPa Show Material materials with Streckgrenze Rp 1,0 of 112 MPa | ||
500.0 °C | 109 MPa Show Material materials with Streckgrenze Rp 1,0 of 109 MPa | ||
550.0 °C | 108 MPa Show Material materials with Streckgrenze Rp 1,0 of 108 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 210 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 450 - 680 MPa Show Material materials with Zugfestigkeit, transversal of 450 - 680 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
200.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
400.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 17.5 - 19.5 % Show Material materials with Chrom of 17.5 - 19.5 % |
Kohlenstoff | 0.03 % Show Material materials with Kohlenstoff of 0.03 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Nickel | 8 - 10 % Show Material materials with Nickel of 8 - 10 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Stickstoff | 0.11 % Show Material materials with Stickstoff of 0.11 % |