General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 0.3 % Show Supplier Material materials with Absorción de agua of 0.3 % | dry | Sim. to ISO 62 |
Densidad | 1.62 g/cm³ Show Supplier Material materials with Densidad of 1.62 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | |
Módulo elástico | 8.5 GPa Show Supplier Material materials with Módulo elástico of 8.5 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 7 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | dry | ISO 179/1eA |
23 °C | 7 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 45 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 45 kJ/m² | dry | ISO 179/1eU |
23 °C | 45 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 45 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 4e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 4e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 5.34e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 5.34e-08 mm²/s | dry | - | |||
Inflamabilidad | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical impact | 120 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 120 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | dry | UL746B | 2 mm | ||
Temperatura de flexión bajo carga | 210 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 210 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 225 °C Show Supplier Material materials with Temperatura de fusión of 225 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.7 [-] Show Supplier Material materials with Constante dieléctrica of 3.7 [-] | dry | IEC 62631-2-1 | 1MHz |
3.9 [-] Show Supplier Material materials with Constante dieléctrica of 3.9 [-] | dry | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 20 [-] Show Supplier Material materials with Factor de disipación of 20 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Factor de disipación of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
Rigidez dieléctrica | 27 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 27 kV/mm | dry | IEC 60243-1 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 250 V Show Supplier Material materials with Índice de seguimiento comparativo of 250 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Density of melt | 1360 g/cm³ Show Supplier Material materials with Density of melt of 1360 g/cm³ | dry | - | |
Specific heat capacity melt | 1870 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1870 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.136 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.136 W/(m·K) | dry | - | |
Velocidad de flujo del volumen derretido | 250 °C | 23 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 23 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Fillers | 20% Glass Fiber |