General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.33 g/cm³ Show Supplier Material materials with Densidad of 1.33 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 3.3 % Show Supplier Material materials with Elongación of 3.3 % | dry | ISO 527-1/-2 |
3.4 % Show Supplier Material materials with Elongación of 3.4 % | dry | ISO 527-1/-2 | ||
13 % Show Supplier Material materials with Elongación of 13 % | conditioned | ISO 527-1/-2 | ||
150 °C | 15 % Show Supplier Material materials with Elongación of 15 % | dry | ISO 527-1/-2 | |
180 °C | 18 % Show Supplier Material materials with Elongación of 18 % | dry | ISO 527-1/-2 | |
200 °C | 19 % Show Supplier Material materials with Elongación of 19 % | dry | ISO 527-1/-2 | |
210 °C | 0.02 % Show Supplier Material materials with Elongación of 0.02 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | conditioned | ISO 178 | |
250 MPa Show Supplier Material materials with Flexural yield strength of 250 MPa | dry | ISO 178 | ||
Módulo de flexión | 3.7 GPa Show Supplier Material materials with Módulo de flexión of 3.7 GPa | conditioned | ISO 178 | |
9 GPa Show Supplier Material materials with Módulo de flexión of 9 GPa | dry | ISO 178 | ||
Módulo elástico | -40 °C | 8.8 GPa Show Supplier Material materials with Módulo elástico of 8.8 GPa | dry | ISO 527-1/-2 |
3.9 GPa Show Supplier Material materials with Módulo elástico of 3.9 GPa | conditioned | ISO 527-1/-2 | ||
8.5 GPa Show Supplier Material materials with Módulo elástico of 8.5 GPa | dry | ISO 527-1/-2 | ||
100 °C | 3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | dry | ISO 527-1/-2 | |
150 °C | 3 GPa Show Supplier Material materials with Módulo elástico of 3 GPa | dry | ISO 527-1/-2 | |
180 °C | 2.6 GPa Show Supplier Material materials with Módulo elástico of 2.6 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.2 GPa Show Supplier Material materials with Módulo elástico of 2.2 GPa | dry | ISO 527-1/-2 | |
210 °C | 2 GPa Show Supplier Material materials with Módulo elástico of 2 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | dry | ISO 527-1/-2 |
85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | conditioned | ISO 527-1/-2 | ||
165 MPa Show Supplier Material materials with Resistencia a la tracción of 165 MPa | dry | ISO 527-1/-2 | ||
100 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | dry | ISO 527-1/-2 | |
150 °C | 75 MPa Show Supplier Material materials with Resistencia a la tracción of 75 MPa | dry | ISO 527-1/-2 | |
180 °C | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | dry | ISO 527-1/-2 | |
200 °C | 55.0 MPa Show Supplier Material materials with Resistencia a la tracción of 55.0 MPa | dry | ISO 527-1/-2 | |
210 °C | 52 MPa Show Supplier Material materials with Resistencia a la tracción of 52 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 7 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | dry | ISO 179/1eA |
23 °C | 13 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
9e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 240 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 240 °C | dry | ISO 75-1/-2 | 2 MPa | |
275 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 275 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 284 °C Show Supplier Material materials with Temperatura de fusión of 284 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 295 °C | 32 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 32 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Hot Charged Air Ducts | |
Fillers | 25% Glass Fiber |