General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 5.5 % Show Supplier Material materials with Absorción de agua of 5.5 % | dry | Sim. to ISO 62 |
Densidad | 1.41 g/cm³ Show Supplier Material materials with Densidad of 1.41 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 3.3 % Show Supplier Material materials with Elongación of 3.3 % | dry | ISO 527-1/-2 |
3.5 % Show Supplier Material materials with Elongación of 3.5 % | dry | ISO 527-1/-2 | ||
5.8 % Show Supplier Material materials with Elongación of 5.8 % | conditioned | ISO 527-1/-2 | ||
120 °C | 7.2 % Show Supplier Material materials with Elongación of 7.2 % | dry | ISO 527-1/-2 | |
140 °C | 7.5 % Show Supplier Material materials with Elongación of 7.5 % | dry | ISO 527-1/-2 | |
150 °C | 8.1 % Show Supplier Material materials with Elongación of 8.1 % | dry | ISO 527-1/-2 | |
160 °C | 8.3 % Show Supplier Material materials with Elongación of 8.3 % | dry | ISO 527-1/-2 | |
180 °C | 8.7 % Show Supplier Material materials with Elongación of 8.7 % | dry | ISO 527-1/-2 | |
200 °C | 9.2 % Show Supplier Material materials with Elongación of 9.2 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 210 MPa Show Supplier Material materials with Flexural yield strength of 210 MPa | conditioned | ISO 178 | |
310 MPa Show Supplier Material materials with Flexural yield strength of 310 MPa | dry | ISO 178 | ||
120 °C | 145 MPa Show Supplier Material materials with Flexural yield strength of 145 MPa | dry | ISO 178 | |
160 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
Módulo de flexión | 7.5 GPa Show Supplier Material materials with Módulo de flexión of 7.5 GPa | conditioned | ISO 178 | |
11 GPa Show Supplier Material materials with Módulo de flexión of 11 GPa | dry | ISO 178 | ||
120 °C | 5.1 GPa Show Supplier Material materials with Módulo de flexión of 5.1 GPa | dry | ISO 178 | |
160 °C | 4.6 GPa Show Supplier Material materials with Módulo de flexión of 4.6 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | ISO 527-1/-2 |
7.5 GPa Show Supplier Material materials with Módulo elástico of 7.5 GPa | conditioned | ISO 527-1/-2 | ||
11.5 GPa Show Supplier Material materials with Módulo elástico of 11.5 GPa | dry | ISO 527-1/-2 | ||
100 °C | 5.7 GPa Show Supplier Material materials with Módulo elástico of 5.7 GPa | dry | ISO 527-1/-2 | |
120 °C | 5.3 GPa Show Supplier Material materials with Módulo elástico of 5.3 GPa | dry | ISO 527-1/-2 | |
140 °C | 5 GPa Show Supplier Material materials with Módulo elástico of 5 GPa | dry | ISO 527-1/-2 | |
150 °C | 4.8 GPa Show Supplier Material materials with Módulo elástico of 4.8 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.6 GPa Show Supplier Material materials with Módulo elástico of 4.6 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.2 GPa Show Supplier Material materials with Módulo elástico of 4.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.9 GPa Show Supplier Material materials with Módulo elástico of 3.9 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 270 MPa Show Supplier Material materials with Resistencia a la tracción of 270 MPa | dry | ISO 527-1/-2 |
140 MPa Show Supplier Material materials with Resistencia a la tracción of 140 MPa | conditioned | ISO 527-1/-2 | ||
210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | dry | ISO 527-1/-2 | ||
100 °C | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | dry | ISO 527-1/-2 | |
120 °C | 111 MPa Show Supplier Material materials with Resistencia a la tracción of 111 MPa | dry | ISO 527-1/-2 | |
140 °C | 101 MPa Show Supplier Material materials with Resistencia a la tracción of 101 MPa | dry | ISO 527-1/-2 | |
150 °C | 98 MPa Show Supplier Material materials with Resistencia a la tracción of 98 MPa | dry | ISO 527-1/-2 | |
160 °C | 94 MPa Show Supplier Material materials with Resistencia a la tracción of 94 MPa | dry | ISO 527-1/-2 | |
180 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
200 °C | 76 MPa Show Supplier Material materials with Resistencia a la tracción of 76 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 12.8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12.8 kJ/m² | dry | ISO 179/1eA | |
23 °C | 18 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 18 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 74 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 74 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 95 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 95 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Inflamabilidad | HB | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical impact | 120 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 120 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical strength | 120 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 120 °C | dry | UL746B | 0.71 mm | ||
Temperatura de flexión bajo carga | 247 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 247 °C | dry | ISO 75-1/-2 | 2 MPa | ||
260 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 260 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.6 [-] Show Supplier Material materials with Constante dieléctrica of 3.6 [-] | dry | IEC 62631-2-1 | 1MHz |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 100Hz | |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
10 [-] Show Supplier Material materials with Constante dieléctrica of 10 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 50 [-] Show Supplier Material materials with Factor de disipación of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
140 [-] Show Supplier Material materials with Factor de disipación of 140 [-] | dry | IEC 62631-2-1 | 1MHz | |
1000 [-] Show Supplier Material materials with Factor de disipación of 1000 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Factor de disipación of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | conditioned | IEC 60243-1 | |
35 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 35 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 500 V Show Supplier Material materials with Índice de seguimiento comparativo of 500 V | dry, conditioned | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | dry | Sim. to ISO 294-4 | Parallel | |
1 % Show Supplier Material materials with Contracción of 1 % | dry | Sim. to ISO 294-4 | Normal | ||
Velocidad de flujo de la masa derretida | 275 °C | 13.3 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 13.3 g/10min | dry | ISO 1133 | |
Velocidad de flujo del volumen derretido | 275 °C | 10.6 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 10.6 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Air inlet manifolds, Integrated Air Inlet Manifolds (up to 180°C), Charge Air Cooler Caps, Fuse Holders, E-Boxes, Automotive Connectors (2) | |
Certifications | Yellow Card Available | |
Fillers | 35% Glass Fiber |