Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 69 % Show Supplier Material materials with Bio-based content of 69 % | dry | ASTM D6866-12 Method B |
Densidad | 1.34 g/cm³ Show Supplier Material materials with Densidad of 1.34 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | |
3.6 % Show Supplier Material materials with Elongación of 3.6 % | conditioned | ISO 527-1/-2 | ||
120 °C | 6.3 % Show Supplier Material materials with Elongación of 6.3 % | dry | ISO 527-1/-2 | |
160 °C | 8.2 % Show Supplier Material materials with Elongación of 8.2 % | dry | ISO 527-1/-2 | |
180 °C | 9.1 % Show Supplier Material materials with Elongación of 9.1 % | dry | ISO 527-1/-2 | |
200 °C | 9.8 % Show Supplier Material materials with Elongación of 9.8 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | conditioned | ISO 178 | |
175 MPa Show Supplier Material materials with Flexural yield strength of 175 MPa | dry | ISO 178 | ||
Módulo de flexión | 4.4 GPa Show Supplier Material materials with Módulo de flexión of 4.4 GPa | conditioned | ISO 178 | |
6.7 GPa Show Supplier Material materials with Módulo de flexión of 6.7 GPa | dry | ISO 178 | ||
Módulo elástico | 6 GPa Show Supplier Material materials with Módulo elástico of 6 GPa | conditioned | ISO 527-1/-2 | |
8 GPa Show Supplier Material materials with Módulo elástico of 8 GPa | dry | ISO 527-1/-2 | ||
120 °C | 2.5 GPa Show Supplier Material materials with Módulo elástico of 2.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 2 GPa Show Supplier Material materials with Módulo elástico of 2 GPa | dry | ISO 527-1/-2 | |
180 °C | 1.6 GPa Show Supplier Material materials with Módulo elástico of 1.6 GPa | dry | ISO 527-1/-2 | |
200 °C | 1.4 GPa Show Supplier Material materials with Módulo elástico of 1.4 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | conditioned | ISO 527-1/-2 | |
95 MPa Show Supplier Material materials with Resistencia a la tracción of 95 MPa | dry | ISO 527-1/-2 | ||
120 °C | 45 MPa Show Supplier Material materials with Resistencia a la tracción of 45 MPa | dry | ISO 527-1/-2 | |
160 °C | 35 MPa Show Supplier Material materials with Resistencia a la tracción of 35 MPa | dry | ISO 527-1/-2 | |
180 °C | 30 MPa Show Supplier Material materials with Resistencia a la tracción of 30 MPa | dry | ISO 527-1/-2 | |
200 °C | 26 MPa Show Supplier Material materials with Resistencia a la tracción of 26 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 4 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4 kJ/m² | dry | ISO 179/1eA |
23 °C | 4 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4 kJ/m² | dry | ISO 179/1eA | |
23 °C | 5.3 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5.3 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 30 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 30 kJ/m² | dry | ISO 179/1eU |
23 °C | 35 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 35 kJ/m² | dry | ISO 179/1eU | |
23 °C | 40 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 40 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 4.8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 4.8e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
7.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 200 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 200 °C | dry | ISO 75-1/-2 | 2 MPa | |
235 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 235 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 250 °C Show Supplier Material materials with Temperatura de fusión of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Engine Covers (close to turbo charged components) | |
Fillers | 30% Glass Fiber and Mineral Powder |