General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.27 g/cm³ Show Supplier Material materials with Densidad of 1.27 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.6 % Show Supplier Material materials with Moisture absorption of 2.6 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3.5 % Show Supplier Material materials with Elongación of 3.5 % | dry | ISO 527-1/-2 | |
20 % Show Supplier Material materials with Elongación of 20 % | conditioned | ISO 527-1/-2 | ||
120 °C | 12 % Show Supplier Material materials with Elongación of 12 % | dry | ISO 527-1/-2 | |
160 °C | 12 % Show Supplier Material materials with Elongación of 12 % | dry | ISO 527-1/-2 | |
200 °C | 13 % Show Supplier Material materials with Elongación of 13 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 85 MPa Show Supplier Material materials with Flexural yield strength of 85 MPa | conditioned | ISO 178 | |
195 MPa Show Supplier Material materials with Flexural yield strength of 195 MPa | dry | ISO 178 | ||
Módulo de flexión | 2.8 GPa Show Supplier Material materials with Módulo de flexión of 2.8 GPa | conditioned | ISO 178 | |
5.7 GPa Show Supplier Material materials with Módulo de flexión of 5.7 GPa | dry | ISO 178 | ||
Módulo elástico | 3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | conditioned | ISO 527-1/-2 | |
7.0 GPa Show Supplier Material materials with Módulo elástico of 7.0 GPa | dry | ISO 527-1/-2 | ||
120 °C | 2.4 GPa Show Supplier Material materials with Módulo elástico of 2.4 GPa | dry | ISO 527-1/-2 | |
160 °C | 2.1 GPa Show Supplier Material materials with Módulo elástico of 2.1 GPa | dry | ISO 527-1/-2 | |
200 °C | 1.6 GPa Show Supplier Material materials with Módulo elástico of 1.6 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 57.0 MPa Show Supplier Material materials with Resistencia a la tracción of 57.0 MPa | conditioned | ISO 527-1/-2 | |
135 MPa Show Supplier Material materials with Resistencia a la tracción of 135 MPa | dry | ISO 527-1/-2 | ||
120 °C | 60 MPa Show Supplier Material materials with Resistencia a la tracción of 60 MPa | dry | ISO 527-1/-2 | |
160 °C | 50 MPa Show Supplier Material materials with Resistencia a la tracción of 50 MPa | dry | ISO 527-1/-2 | |
200 °C | 37 MPa Show Supplier Material materials with Resistencia a la tracción of 37 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 3 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 3 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 14.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 14.0 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 41 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 41 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 63 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 63 kJ/m² | dry | ISO 179/1eU | |
23 °C | 74 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 74 kJ/m² | dry | ISO 179/1eU | |
23 °C | 95 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 95 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Temperatura de flexión bajo carga | 218 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 218 °C | dry | ISO 75-1/-2 | 2 MPa | |
Temperatura de fusión | 255 °C Show Supplier Material materials with Temperatura de fusión of 255 °C | dry | ISO 11357-1/-3 | 10°C/min |
Technological properties
Property | ||
---|---|---|
Fillers | 20% Glass Fiber |