General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.18 g/cm³ Show Supplier Material materials with Densidad of 1.18 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dureza Shore D | 37 [-] Show Supplier Material materials with Dureza Shore D of 37 [-] | dry | ISO 868 | 3s |
Elongación | 160 % Show Supplier Material materials with Elongación of 160 % | dry | ISO 527-1/-2 | |
760 % Show Supplier Material materials with Elongación of 760 % | dry | ISO 527-1/-2 | ||
Módulo elástico | 0.07 GPa Show Supplier Material materials with Módulo elástico of 0.07 GPa | dry | ISO 527-1/-2 | |
Resistencia a desgarros | 91 kN/m Show Supplier Material materials with Resistencia a desgarros of 91 kN/m | dry | ISO 34-1; Method B | |
104 kN/m Show Supplier Material materials with Resistencia a desgarros of 104 kN/m | dry | ISO 34-1; Method B | ||
Resistencia a la tracción | 16 MPa Show Supplier Material materials with Resistencia a la tracción of 16 MPa | dry | ISO 527-1/-2 | |
27 MPa Show Supplier Material materials with Resistencia a la tracción of 27 MPa | dry | ISO 527-1/-2 | Normal |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Temperatura de flexión bajo carga | 65 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 65 °C | dry | ISO 75-1/-2 | 0.45 MPa | |
Temperatura de fusión | 212 °C Show Supplier Material materials with Temperatura de fusión of 212 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | -60 °C Show Supplier Material materials with Temperatura de transición del vidrio of -60 °C | dry | ISO 11357-1/-2 | 10°C/min |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 1.5 % Show Supplier Material materials with Contracción of 1.5 % | dry | Sim. to ISO 294-4 | Parallel | |
2.3 % Show Supplier Material materials with Contracción of 2.3 % | dry | Sim. to ISO 294-4 | Normal | ||
Velocidad de flujo del volumen derretido | 230 °C | 11 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 11 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Boots and Bellows |