General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 0.6 % Show Supplier Material materials with Absorción de agua of 0.6 % | dry | Sim. to ISO 62 |
Densidad | 1.29 g/cm³ Show Supplier Material materials with Densidad of 1.29 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Mecánica
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dureza Shore D | 71 [-] Show Supplier Material materials with Dureza Shore D of 71 [-] | dry | ISO 868 | 3s |
Elongación | 300 % Show Supplier Material materials with Elongación of 300 % | dry | ISO 527-1/-2 | |
360 % Show Supplier Material materials with Elongación of 360 % | dry | ISO 527-1/-2 | ||
570 % Show Supplier Material materials with Elongación of 570 % | dry | ISO 527-1/-2 | ||
Módulo de flexión | 0.94 GPa Show Supplier Material materials with Módulo de flexión of 0.94 GPa | dry | ISO 178 | |
Módulo elástico | 0.9 GPa Show Supplier Material materials with Módulo elástico of 0.9 GPa | dry | ISO 527-1/-2 | |
Resistencia a desgarros | 224 kN/m Show Supplier Material materials with Resistencia a desgarros of 224 kN/m | dry | ISO 34-1; Method B | |
228 kN/m Show Supplier Material materials with Resistencia a desgarros of 228 kN/m | dry | ISO 34-1; Method B | ||
Resistencia a la tracción | 45 MPa Show Supplier Material materials with Resistencia a la tracción of 45 MPa | dry | ISO 527-1/-2 | |
58.0 MPa Show Supplier Material materials with Resistencia a la tracción of 58.0 MPa | dry | ISO 527-1/-2 | Normal |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Temperatura de fusión | 221 °C Show Supplier Material materials with Temperatura de fusión of 221 °C | dry | ISO 11357-1/-3 | 10°C/min |
Temperatura de transición del vidrio | 110 °C Show Supplier Material materials with Temperatura de transición del vidrio of 110 °C | dry | ASTM D5026/D7028 | DMTA (E) |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 62631-2-1 | 1MHz |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 230 °C | 4 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 4 cm³/10min | dry | ISO 1133 |
Technological properties
Property |
---|