General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 8.5 % Show Supplier Material materials with Absorción de agua of 8.5 % | dry | Sim. to ISO 62 |
Densidad | 1.14 g/cm³ Show Supplier Material materials with Densidad of 1.14 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 10 % Show Supplier Material materials with Elongación of 10 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Elongación of 50 % | conditioned | ISO 527-1/-2 | ||
Elongation at yield | 3.5 % Show Supplier Material materials with Elongation at yield of 3.5 % | dry | ISO 527-1/-2 | |
20 % Show Supplier Material materials with Elongation at yield of 20 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 125 MPa Show Supplier Material materials with Flexural yield strength of 125 MPa | dry | ISO 178 | |
Módulo de flexión | 2.8 GPa Show Supplier Material materials with Módulo de flexión of 2.8 GPa | dry | ISO 178 | |
Módulo elástico | 1.5 GPa Show Supplier Material materials with Módulo elástico of 1.5 GPa | conditioned | ISO 527-1/-2 | |
3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | conditioned | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1e-06 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1e-06 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 4.87e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 4.87e-08 mm²/s | dry | - | |||
Inflamabilidad | V-2 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical impact | 100 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 100 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.71 mm | ||
Temperatura de flexión bajo carga | 85 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 85 °C | dry | ISO 75-1/-2 | 2 MPa | ||
215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3 [-] Show Supplier Material materials with Constante dieléctrica of 3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.2 [-] Show Supplier Material materials with Constante dieléctrica of 3.2 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.3 [-] Show Supplier Material materials with Constante dieléctrica of 4.3 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
15 [-] Show Supplier Material materials with Constante dieléctrica of 15 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 60 [-] Show Supplier Material materials with Factor de disipación of 60 [-] | dry | IEC 62631-2-1 | 100Hz |
170 [-] Show Supplier Material materials with Factor de disipación of 170 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Factor de disipación of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
2400 [-] Show Supplier Material materials with Factor de disipación of 2400 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 25 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | dry, conditioned | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.95 % Show Supplier Material materials with Contracción of 0.95 % | dry | ISO 294-4 | Parallel |
0.95 % Show Supplier Material materials with Contracción of 0.95 % | dry | ISO 294-4 | Normal | |
Density of melt | 969 g/cm³ Show Supplier Material materials with Density of melt of 969 g/cm³ | dry | - | |
Specific heat capacity melt | 2750 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2750 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.13 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.13 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available |