General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.49 g/cm³ Show Supplier Material materials with Densidad of 1.49 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
5 % Show Supplier Material materials with Elongación of 5 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 250 MPa Show Supplier Material materials with Flexural yield strength of 250 MPa | conditioned | ISO 178 | |
355 MPa Show Supplier Material materials with Flexural yield strength of 355 MPa | dry | ISO 178 | ||
Módulo de flexión | 9 GPa Show Supplier Material materials with Módulo de flexión of 9 GPa | conditioned | ISO 178 | |
13.6 GPa Show Supplier Material materials with Módulo de flexión of 13.6 GPa | dry | ISO 178 | ||
Módulo elástico | 9 GPa Show Supplier Material materials with Módulo elástico of 9 GPa | conditioned | ISO 527-1/-2 | |
13.6 GPa Show Supplier Material materials with Módulo elástico of 13.6 GPa | dry | ISO 527-1/-2 | ||
Resistencia a la tracción | 150 MPa Show Supplier Material materials with Resistencia a la tracción of 150 MPa | conditioned | ISO 527-1/-2 | |
220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | 23 °C | 18 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 18 kJ/m² | dry | ISO 179/1eA |
23 °C | 27 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 27 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 110 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 110 kJ/m² | dry | ISO 179/1eU |
23 °C | 120 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 120 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Temperatura de flexión bajo carga | 209 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 209 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
5 [-] Show Supplier Material materials with Constante dieléctrica of 5 [-] | dry | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 240 [-] Show Supplier Material materials with Factor de disipación of 240 [-] | dry | IEC 62631-2-1 | 1MHz |
280 [-] Show Supplier Material materials with Factor de disipación of 280 [-] | dry | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 27 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 27 kV/mm | dry | IEC 60243-1 | |
Surface resistivity | 3e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 3e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 2e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+12 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 400 V Show Supplier Material materials with Índice de seguimiento comparativo of 400 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | dry | ISO 294-4 | Parallel | |
0.8 % Show Supplier Material materials with Contracción of 0.8 % | dry | ISO 294-4 | Normal | ||
Velocidad de flujo de la masa derretida | 250 °C | 4 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 4 g/10min | dry | ISO 1133 | |
Velocidad de flujo del volumen derretido | 250 °C | 3 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 3 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Fillers | 45% Glass Fiber |