General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 8.5 % Show Supplier Material materials with Absorción de agua of 8.5 % | dry | Sim. to ISO 62 |
Densidad | 1.14 g/cm³ Show Supplier Material materials with Densidad of 1.14 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 10 % Show Supplier Material materials with Elongación of 10 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Elongación of 50 % | conditioned | ISO 527-1/-2 | ||
Elongation at yield | 3.5 % Show Supplier Material materials with Elongation at yield of 3.5 % | dry | ISO 527-1/-2 | |
20 % Show Supplier Material materials with Elongation at yield of 20 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 125 MPa Show Supplier Material materials with Flexural yield strength of 125 MPa | dry | ISO 178 | |
Módulo de flexión | 2.8 GPa Show Supplier Material materials with Módulo de flexión of 2.8 GPa | dry | ISO 178 | |
Módulo elástico | 1.5 GPa Show Supplier Material materials with Módulo elástico of 1.5 GPa | conditioned | ISO 527-1/-2 | |
3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | conditioned | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 85 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 85 °C | dry | ISO 75-1/-2 | 2 MPa | |
215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Property | Value | Condition | Testing Standard |
---|---|---|---|
Viscosity number | 130 cm³/gr Show Supplier Material materials with Viscosity number of 130 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Certifications | Food Contact |