Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.62 g/cm³ Show Supplier Material materials with Densidad of 1.62 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 285 MPa Show Supplier Material materials with Flexural yield strength of 285 MPa | dry | ISO 178 | |
Módulo de flexión | 11.5 GPa Show Supplier Material materials with Módulo de flexión of 11.5 GPa | dry | ISO 178 | |
Módulo elástico | 12.5 GPa Show Supplier Material materials with Módulo elástico of 12.5 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 200 MPa Show Supplier Material materials with Resistencia a la tracción of 200 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | 23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry | ISO 179/1eA |
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
5.3e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5.3e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 3 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 3 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 3 mm | ||
Temperatura de flexión bajo carga | 270 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 270 °C | dry | ISO 75-1/-2 | 2 MPa | ||
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Índice de seguimiento comparativo | 200 V Show Supplier Material materials with Índice de seguimiento comparativo of 200 V | dry | IEC 60112 |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available | |
Fillers | 33% Glass Fiber |