General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 70 % Show Supplier Material materials with Bio-based content of 70 % | dry | ASTM D6866-12 Method B |
Densidad | 1.34 g/cm³ Show Supplier Material materials with Densidad of 1.34 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3.8 % Show Supplier Material materials with Elongación of 3.8 % | dry | ISO 527-1/-2 | |
5.8 % Show Supplier Material materials with Elongación of 5.8 % | conditioned | ISO 527-1/-2 | ||
120 °C | 8.2 % Show Supplier Material materials with Elongación of 8.2 % | dry | ISO 527-1/-2 | |
160 °C | 9.4 % Show Supplier Material materials with Elongación of 9.4 % | dry | ISO 527-1/-2 | |
180 °C | 10 % Show Supplier Material materials with Elongación of 10 % | dry | ISO 527-1/-2 | |
200 °C | 10 % Show Supplier Material materials with Elongación of 10 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 185 MPa Show Supplier Material materials with Flexural yield strength of 185 MPa | conditioned | ISO 178 | |
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||
120 °C | 145 MPa Show Supplier Material materials with Flexural yield strength of 145 MPa | dry | ISO 178 | |
Módulo de flexión | 6.3 GPa Show Supplier Material materials with Módulo de flexión of 6.3 GPa | conditioned | ISO 178 | |
8.5 GPa Show Supplier Material materials with Módulo de flexión of 8.5 GPa | dry | ISO 178 | ||
120 °C | 4.8 GPa Show Supplier Material materials with Módulo de flexión of 4.8 GPa | dry | ISO 178 | |
Módulo elástico | 7 GPa Show Supplier Material materials with Módulo elástico of 7 GPa | conditioned | ISO 527-1/-2 | |
9.2 GPa Show Supplier Material materials with Módulo elástico of 9.2 GPa | dry | ISO 527-1/-2 | ||
120 °C | 4.6 GPa Show Supplier Material materials with Módulo elástico of 4.6 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.7 GPa Show Supplier Material materials with Módulo elástico of 3.7 GPa | dry | ISO 527-1/-2 | |
180 °C | 3.2 GPa Show Supplier Material materials with Módulo elástico of 3.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 3 GPa Show Supplier Material materials with Módulo elástico of 3 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | |
170 MPa Show Supplier Material materials with Resistencia a la tracción of 170 MPa | dry | ISO 527-1/-2 | ||
120 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
160 °C | 70 MPa Show Supplier Material materials with Resistencia a la tracción of 70 MPa | dry | ISO 527-1/-2 | |
180 °C | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | dry | ISO 527-1/-2 | |
200 °C | 60 MPa Show Supplier Material materials with Resistencia a la tracción of 60 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | dry | ISO 179/1eA |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry | ISO 179/1eA | |
23 °C | 15 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | dry | ISO 179/1eU |
23 °C | 80 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 80 kJ/m² | dry, conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 3.2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3.2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6.6e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 6.6e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | dry | ISO 75-1/-2 | 2 MPa | |
243 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 243 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 250 °C Show Supplier Material materials with Temperatura de fusión of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | dry | ISO 294-4 | Parallel | |
1 % Show Supplier Material materials with Contracción of 1 % | dry | ISO 294-4 | Normal | ||
Velocidad de flujo de la masa derretida | 290 °C | 42 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 42 g/10min | dry | ISO 1133 | |
Velocidad de flujo del volumen derretido | 290 °C | 36 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 36 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Window profiles, Snowboard bindings, Mountaineering shoes, Coolant Hose T-Connectors, Charge Air Cooler Caps, Fuel System: Various Components, Fuel Line Connectors, Automotive Connectors, Temperature Sensor, Speed Sensor, Positition Sensor, Wheel Speed Sensors, Coolant expansion tank, Radiator end tanks, Coolant connectors | |
Fillers | 30% Glass Fiber |