General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 5 % Show Supplier Material materials with Absorción de agua of 5 % | dry | Sim. to ISO 62 |
Densidad | 1.5 g/cm³ Show Supplier Material materials with Densidad of 1.5 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.3 % Show Supplier Material materials with Moisture absorption of 1.3 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-1/-2 | |
4 % Show Supplier Material materials with Elongación of 4 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 330 MPa Show Supplier Material materials with Flexural yield strength of 330 MPa | dry | ISO 178 | |
Módulo de flexión | 11.9 GPa Show Supplier Material materials with Módulo de flexión of 11.9 GPa | dry | ISO 178 | |
Módulo elástico | 9.5 GPa Show Supplier Material materials with Módulo elástico of 9.5 GPa | conditioned | ISO 527-1/-2 | |
13 GPa Show Supplier Material materials with Módulo elástico of 13 GPa | dry | ISO 527-1/-2 | ||
Resistencia a la tracción | 160 MPa Show Supplier Material materials with Resistencia a la tracción of 160 MPa | conditioned | ISO 527-1/-2 | |
210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | dry | ISO 179/1eA |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 18 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 18 kJ/m² | conditioned | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Inflamabilidad | HB | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 2 mm | ||
Temperatura de flexión bajo carga | 250 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 250 °C | dry | ISO 75-1/-2 | 2 MPa | ||
260 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 260 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available | |
Fillers | 42% Glass Fiber and MoS2 |