General
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2.2 % Show Supplier Material materials with Elongación of 2.2 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 255 MPa Show Supplier Material materials with Flexural yield strength of 255 MPa | dry | ISO 178 | |
Módulo de flexión | 14 GPa Show Supplier Material materials with Módulo de flexión of 14 GPa | dry | ISO 178 | |
Módulo elástico | 15 GPa Show Supplier Material materials with Módulo elástico of 15 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 180 MPa Show Supplier Material materials with Resistencia a la tracción of 180 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | 23 °C | 13 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | dry | ISO 179/1eA |
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 70 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 70 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 3 mm | IEC 60695-2-12 | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 0.8 mm | IEC 60695-2-12 | |||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | 2 mm | IEC 60695-2-13 | ||
825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | 3 mm | IEC 60695-2-13 | |||
Temperatura de flexión bajo carga | 276 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 276 °C | dry | ISO 75-1/-2 | 2 MPa | ||
282 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 282 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 286 °C Show Supplier Material materials with Temperatura de fusión of 286 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4.2 [-] Show Supplier Material materials with Constante dieléctrica of 4.2 [-] | dry | IEC 60250 | 1GHz |
4.4 [-] Show Supplier Material materials with Constante dieléctrica of 4.4 [-] | conditioned | IEC 60250 | 1GHz | |
Factor de disipación | 100 [-] Show Supplier Material materials with Factor de disipación of 100 [-] | dry | IEC 60250 | 1GHz |
160 [-] Show Supplier Material materials with Factor de disipación of 160 [-] | conditioned | IEC 60250 | 1GHz | |
Rigidez dieléctrica | 40 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 40 kV/mm | dry | IEC 60243-1 | |
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.3 % Show Supplier Material materials with Contracción of 0.3 % | dry | ISO 294-4 | Parallel |
0.9 % Show Supplier Material materials with Contracción of 0.9 % | dry | ISO 294-4 | Normal | |
Spiral flow length | 125 | dry | - | 1.0 mm 800 bar |
137 | dry | - | 1.0 mm 900 bar | |
150 | dry | - | 1.0 mm 1000 bar |
Technological properties
Property | ||
---|---|---|
Application areas | USB-C Connectors, DDR DIMM Connectors | |
Certifications | Yellow Card Available | |
Fillers | 45% Glass Fiber |