General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 0.4 % Show Supplier Material materials with Absorción de agua of 0.4 % | dry | Sim. to ISO 62 |
Densidad | 1.59 g/cm³ Show Supplier Material materials with Densidad of 1.59 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 |
2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | ||
120 °C | 6 % Show Supplier Material materials with Elongación of 6 % | dry | ISO 527-1/-2 | |
160 °C | 7 % Show Supplier Material materials with Elongación of 7 % | dry | ISO 527-1/-2 | |
180 °C | 7.5 % Show Supplier Material materials with Elongación of 7.5 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 165 MPa Show Supplier Material materials with Flexural yield strength of 165 MPa | dry | ISO 178 | |
120 °C | 85 MPa Show Supplier Material materials with Flexural yield strength of 85 MPa | dry | ISO 178 | |
160 °C | 65 MPa Show Supplier Material materials with Flexural yield strength of 65 MPa | dry | ISO 178 | |
Módulo de flexión | 7.7 GPa Show Supplier Material materials with Módulo de flexión of 7.7 GPa | dry | ISO 178 | |
120 °C | 3.4 GPa Show Supplier Material materials with Módulo de flexión of 3.4 GPa | dry | ISO 178 | |
160 °C | 2.7 GPa Show Supplier Material materials with Módulo de flexión of 2.7 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 9.5 GPa Show Supplier Material materials with Módulo elástico of 9.5 GPa | dry | ISO 527-1/-2 |
8.2 GPa Show Supplier Material materials with Módulo elástico of 8.2 GPa | dry | ISO 527-1/-2 | ||
100 °C | 3.9 GPa Show Supplier Material materials with Módulo elástico of 3.9 GPa | dry | ISO 527-1/-2 | |
120 °C | 3.5 GPa Show Supplier Material materials with Módulo elástico of 3.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 2.8 GPa Show Supplier Material materials with Módulo elástico of 2.8 GPa | dry | ISO 527-1/-2 | |
180 °C | 2.4 GPa Show Supplier Material materials with Módulo elástico of 2.4 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 150 MPa Show Supplier Material materials with Resistencia a la tracción of 150 MPa | dry | ISO 527-1/-2 |
110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | dry | ISO 527-1/-2 | ||
100 °C | 60 MPa Show Supplier Material materials with Resistencia a la tracción of 60 MPa | dry | ISO 527-1/-2 | |
120 °C | 55.0 MPa Show Supplier Material materials with Resistencia a la tracción of 55.0 MPa | dry | ISO 527-1/-2 | |
160 °C | 45 MPa Show Supplier Material materials with Resistencia a la tracción of 45 MPa | dry | ISO 527-1/-2 | |
180 °C | 40 MPa Show Supplier Material materials with Resistencia a la tracción of 40 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | dry | ISO 179/1eA |
23 °C | 7 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry | ISO 179/1eU |
23 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 4e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 4e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 5.34e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 5.34e-08 mm²/s | dry | - | |||
Inflamabilidad | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | dry | UL746B | 0.75 mm | ||
Temperatura de flexión bajo carga | 210 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 210 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 225 °C Show Supplier Material materials with Temperatura de fusión of 225 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.2 [-] Show Supplier Material materials with Constante dieléctrica of 3.2 [-] | dry | IEC 62631-2-1 | 100Hz |
3.2 [-] Show Supplier Material materials with Constante dieléctrica of 3.2 [-] | dry | IEC 62631-2-1 | 1MHz | |
Factor de disipación | 10 [-] Show Supplier Material materials with Factor de disipación of 10 [-] | dry | IEC 62631-2-1 | 100Hz |
140 [-] Show Supplier Material materials with Factor de disipación of 140 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 225 V Show Supplier Material materials with Índice de seguimiento comparativo of 225 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Density of melt | 1360 g/cm³ Show Supplier Material materials with Density of melt of 1360 g/cm³ | dry | - | |
Specific heat capacity melt | 1870 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1870 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.136 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.136 W/(m·K) | dry | - | |
Velocidad de flujo de la masa derretida | 250 °C | 25 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 25 g/10min | dry | ISO 1133 |
Velocidad de flujo del volumen derretido | 250 °C | 19 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 19 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Fuse Holders, E-Boxes, Automotive Connectors (3) | |
Certifications | Yellow Card Available | |
Fillers | 20% Glass Fiber |