General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 6.5 % Show Supplier Material materials with Absorción de agua of 6.5 % | dry | Sim. to ISO 62 |
Densidad | 1.34 g/cm³ Show Supplier Material materials with Densidad of 1.34 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2 % Show Supplier Material materials with Moisture absorption of 2 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
Módulo elástico | 4.8 GPa Show Supplier Material materials with Módulo elástico of 4.8 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 63 MPa Show Supplier Material materials with Resistencia a la tracción of 63 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | 23 °C | 2 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 2 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|
Ball pressure temperature | 200 °C Show Supplier Material materials with Ball pressure temperature of 200 °C | dry | IEC 60695-10-2 | ||
Inflamabilidad | V-2 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.8 mm | |
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.8 mm | |
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 62631-2-1 | 1MHz |
3.9 [-] Show Supplier Material materials with Constante dieléctrica of 3.9 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
4.3 [-] Show Supplier Material materials with Constante dieléctrica of 4.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
10 [-] Show Supplier Material materials with Constante dieléctrica of 10 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 130 [-] Show Supplier Material materials with Factor de disipación of 130 [-] | dry | IEC 62631-2-1 | 100Hz |
210 [-] Show Supplier Material materials with Factor de disipación of 210 [-] | dry | IEC 62631-2-1 | 1MHz | |
1000 [-] Show Supplier Material materials with Factor de disipación of 1000 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Factor de disipación of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 25 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Molded case circuit breakers | |
Certifications | Yellow Card Available | |
Fillers | 20% Glass Fiber |