General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 5.7 % Show Supplier Material materials with Absorción de agua of 5.7 % | dry | Sim. to ISO 62 |
Densidad | 1.41 g/cm³ Show Supplier Material materials with Densidad of 1.41 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3.5 % Show Supplier Material materials with Elongación of 3.5 % | dry | ISO 527-1/-2 | |
7 % Show Supplier Material materials with Elongación of 7 % | conditioned | ISO 527-1/-2 | ||
Módulo elástico | 7.3 GPa Show Supplier Material materials with Módulo elástico of 7.3 GPa | conditioned | ISO 527-1/-2 | |
11.5 GPa Show Supplier Material materials with Módulo elástico of 11.5 GPa | dry | ISO 527-1/-2 | ||
Resistencia a la tracción | 110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | conditioned | ISO 527-1/-2 | |
175 MPa Show Supplier Material materials with Resistencia a la tracción of 175 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 13 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 20 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 20 kJ/m² | dry | ISO 179/1eA | |
23 °C | 30 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 30 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU |
-30 °C | 95 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 95 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 100 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 6.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 200 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 200 °C | dry | ISO 75-1/-2 | 2 MPa | |
215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.3 [-] Show Supplier Material materials with Constante dieléctrica of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Constante dieléctrica of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Constante dieléctrica of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 90 [-] Show Supplier Material materials with Factor de disipación of 90 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Factor de disipación of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Factor de disipación of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Factor de disipación of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 20 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 20 kV/mm | conditioned | IEC 60243-1 | |
25 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 25 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | conditioned | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 0.36 % Show Supplier Material materials with Contracción of 0.36 % | dry | ISO 294-4 | Parallel | |
0.89 % Show Supplier Material materials with Contracción of 0.89 % | dry | ISO 294-4 | Normal | ||
Velocidad de flujo de la masa derretida | 75 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 75 g/10min | dry | ISO 1133 | ||
Velocidad de flujo del volumen derretido | 275 °C | 60 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 60 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Airbag Containers | |
Fillers | 40% Glass Fiber |