General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.05 % Show Supplier Material materials with Absorción de agua of 0.05 % | dry | ISO 62 | at 23°C after 24h |
Densidad | 1.55 g/cm³ Show Supplier Material materials with Densidad of 1.55 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.05 % Show Supplier Material materials with Moisture absorption of 0.05 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dureza Rockwell M | 100 [-] Show Supplier Material materials with Dureza Rockwell M of 100 [-] | dry | ISO 2039-2 | |
Elongación | -40 °C | 2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-1/-2 | ||
120 °C | 4.6 % Show Supplier Material materials with Elongación of 4.6 % | dry | ISO 527-1/-2 | |
160 °C | 5.3 % Show Supplier Material materials with Elongación of 5.3 % | dry | ISO 527-1/-2 | |
200 °C | 5.4 % Show Supplier Material materials with Elongación of 5.4 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 240 MPa Show Supplier Material materials with Flexural yield strength of 240 MPa | dry | ISO 178 | |
120 °C | 96 MPa Show Supplier Material materials with Flexural yield strength of 96 MPa | dry | ISO 178 | |
160 °C | 68 MPa Show Supplier Material materials with Flexural yield strength of 68 MPa | dry | ISO 178 | |
200 °C | 56.0 MPa Show Supplier Material materials with Flexural yield strength of 56.0 MPa | dry | ISO 178 | |
Hardness, Rockwell R | 120 [-] Show Supplier Material materials with Hardness, Rockwell R of 120 [-] | dry | ISO 2039-2 | |
Módulo de flexión | 10 GPa Show Supplier Material materials with Módulo de flexión of 10 GPa | dry | ISO 178 | |
120 °C | 4.5 GPa Show Supplier Material materials with Módulo de flexión of 4.5 GPa | dry | ISO 178 | |
160 °C | 3.3 GPa Show Supplier Material materials with Módulo de flexión of 3.3 GPa | dry | ISO 178 | |
200 °C | 2.9 GPa Show Supplier Material materials with Módulo de flexión of 2.9 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | ISO 527-1/-2 |
12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | ISO 527-1/-2 | ||
120 °C | 4.7 GPa Show Supplier Material materials with Módulo elástico of 4.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.5 GPa Show Supplier Material materials with Módulo elástico of 3.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.0 GPa Show Supplier Material materials with Módulo elástico of 3.0 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 185 MPa Show Supplier Material materials with Resistencia a la tracción of 185 MPa | dry | ISO 527-1/-2 |
170 MPa Show Supplier Material materials with Resistencia a la tracción of 170 MPa | dry | ISO 527-1/-2 | ||
120 °C | 70 MPa Show Supplier Material materials with Resistencia a la tracción of 70 MPa | dry | ISO 527-1/-2 | |
160 °C | 55.0 MPa Show Supplier Material materials with Resistencia a la tracción of 55.0 MPa | dry | ISO 527-1/-2 | |
200 °C | 45 MPa Show Supplier Material materials with Resistencia a la tracción of 45 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | dry | ISO 179/1eA |
23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 56.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 56.0 kJ/m² | dry | ISO 179/1eU |
23 °C | 58.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 58.0 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.8e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1.8e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.8e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | |||
5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
1.2e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.2e-06 1/K | dry | ISO 11359-1/-2 | normal, above Tg | |||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.4 mm | ||
Temperatura de flexión bajo carga | 185 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 185 °C | dry | ISO 75-1/-2 | 8 MPa | ||
265 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 265 °C | dry | ISO 75-1/-2 | 2 MPa | |||
280 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 280 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 280 °C Show Supplier Material materials with Temperatura de fusión of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de transición del vidrio | 90 °C Show Supplier Material materials with Temperatura de transición del vidrio of 90 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 60250 | 1GHz |
3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 60250 | 5GHz | |
Factor de disipación | 30 [-] Show Supplier Material materials with Factor de disipación of 30 [-] | dry | IEC 60250 | 1GHz |
45 [-] Show Supplier Material materials with Factor de disipación of 45 [-] | dry | IEC 60250 | 5GHz | |
Rigidez dieléctrica | 34 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 34 kV/mm | dry | IEC 60243-1 | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 175 V Show Supplier Material materials with Índice de seguimiento comparativo of 175 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | ADAS Radar Housing | |
Fillers | 30% Glass Fiber |