General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.18 % Show Supplier Material materials with Absorción de agua of 0.18 % | dry | ISO 62 | at 23°C after 24h |
Densidad | 1.32 g/cm³ Show Supplier Material materials with Densidad of 1.32 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.1 % Show Supplier Material materials with Moisture absorption of 0.1 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dureza Shore A | 98 [-] Show Supplier Material materials with Dureza Shore A of 98 [-] | dry | ISO 868 | 15s | |
99 [-] Show Supplier Material materials with Dureza Shore A of 99 [-] | dry | ISO 868 | 3s | ||
Dureza Shore D | 62 [-] Show Supplier Material materials with Dureza Shore D of 62 [-] | dry | ISO 868 | 3s | |
62 [-] Show Supplier Material materials with Dureza Shore D of 62 [-] | dry | ISO 868 | 15s | ||
Elongación | 50 % Show Supplier Material materials with Elongación of 50 % | dry | ISO 527-1/-2 | ||
Elongation at yield | 18 % Show Supplier Material materials with Elongation at yield of 18 % | dry | ISO 527-1/-2 | ||
Módulo elástico | 0.54 GPa Show Supplier Material materials with Módulo elástico of 0.54 GPa | dry | ISO 527-1/-2 | ||
Resistencia a desgarros | 132 kN/m Show Supplier Material materials with Resistencia a desgarros of 132 kN/m | dry | ISO 34-1; Method B | ||
Resistencia a la tracción | 20.5 MPa Show Supplier Material materials with Resistencia a la tracción of 20.5 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 3 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 3 kJ/m² | dry | ISO 179/1eA | |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Temperatura de fusión | 205 °C Show Supplier Material materials with Temperatura de fusión of 205 °C | dry | ISO 11357-1/-3 | 10°C/min |
Temperatura de reblandecimiento Vicat | 85 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 85 °C | dry | ISO 306 | 50°C/h 50N |
Temperatura de transición del vidrio | -10 °C Show Supplier Material materials with Temperatura de transición del vidrio of -10 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.7 [-] Show Supplier Material materials with Constante dieléctrica of 3.7 [-] | dry | IEC 62631-2-1 | 1MHz |
4.2 [-] Show Supplier Material materials with Constante dieléctrica of 4.2 [-] | dry | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 157 [-] Show Supplier Material materials with Factor de disipación of 157 [-] | dry | IEC 62631-2-1 | 100Hz |
385 [-] Show Supplier Material materials with Factor de disipación of 385 [-] | dry | IEC 62631-2-1 | 1MHz | |
Rigidez dieléctrica | 18.7 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 18.7 kV/mm | dry | IEC 60243-1 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 230 °C | 13 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 13 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Wire and Cable Insulation | |
Certifications | Yellow Card Available |