General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 5.7 % Show Supplier Material materials with Absorción de agua of 5.7 % | dry | Sim. to ISO 62 |
Densidad | 1.32 g/cm³ Show Supplier Material materials with Densidad of 1.32 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 5 % Show Supplier Material materials with Elongación of 5 % | dry | ISO 527-1/-2 |
5 % Show Supplier Material materials with Elongación of 5 % | dry | ISO 527-1/-2 | ||
10 % Show Supplier Material materials with Elongación of 10 % | conditioned | ISO 527-1/-2 | ||
120 °C | 14.3 % Show Supplier Material materials with Elongación of 14.3 % | dry | ISO 527-1/-2 | |
150 °C | 15.2 % Show Supplier Material materials with Elongación of 15.2 % | dry | ISO 527-1/-2 | |
160 °C | 15.5 % Show Supplier Material materials with Elongación of 15.5 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | conditioned | ISO 178 | |
250 MPa Show Supplier Material materials with Flexural yield strength of 250 MPa | dry | ISO 178 | ||
Módulo de flexión | 4.9 GPa Show Supplier Material materials with Módulo de flexión of 4.9 GPa | conditioned | ISO 178 | |
8.5 GPa Show Supplier Material materials with Módulo de flexión of 8.5 GPa | dry | ISO 178 | ||
Módulo elástico | 4.8 GPa Show Supplier Material materials with Módulo elástico of 4.8 GPa | conditioned | ISO 527-1/-2 | |
8.7 GPa Show Supplier Material materials with Módulo elástico of 8.7 GPa | dry | ISO 527-1/-2 | ||
40 °C | 8.9 GPa Show Supplier Material materials with Módulo elástico of 8.9 GPa | dry | ISO 527-1/-2 | |
100 °C | 3.7 GPa Show Supplier Material materials with Módulo elástico of 3.7 GPa | dry | ISO 527-1/-2 | |
120 °C | 3.5 GPa Show Supplier Material materials with Módulo elástico of 3.5 GPa | dry | ISO 527-1/-2 | |
150 °C | 3.1 GPa Show Supplier Material materials with Módulo elástico of 3.1 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.0 GPa Show Supplier Material materials with Módulo elástico of 3.0 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 235 MPa Show Supplier Material materials with Resistencia a la tracción of 235 MPa | dry | ISO 527-1/-2 |
105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | conditioned | ISO 527-1/-2 | ||
150 MPa Show Supplier Material materials with Resistencia a la tracción of 150 MPa | dry | ISO 527-1/-2 | ||
100 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
120 °C | 80 MPa Show Supplier Material materials with Resistencia a la tracción of 80 MPa | dry | ISO 527-1/-2 | |
150 °C | 70 MPa Show Supplier Material materials with Resistencia a la tracción of 70 MPa | dry | ISO 527-1/-2 | |
160 °C | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 15 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 23 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 23 kJ/m² | dry | ISO 179/1eA | |
23 °C | 43 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 43 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 100 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 100 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 95 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 95 kJ/m² | dry | ISO 179/1eU | |
23 °C | 110 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 110 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
9e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 8.99e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 8.99e-08 mm²/s | dry | - | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm | ||
Temperatura de flexión bajo carga | 200 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 200 °C | dry | ISO 75-1/-2 | 2 MPa | ||
215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.5 [-] Show Supplier Material materials with Constante dieléctrica of 3.5 [-] | dry | IEC 62631-2-1 | 1MHz |
3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Constante dieléctrica of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 90 [-] Show Supplier Material materials with Factor de disipación of 90 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Factor de disipación of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Factor de disipación of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Factor de disipación of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 20 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 20 kV/mm | conditioned | IEC 60243-1 | |
25 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 25 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | conditioned | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 0.39 % Show Supplier Material materials with Contracción of 0.39 % | dry | ISO 294-4 | Parallel | |
1 % Show Supplier Material materials with Contracción of 1 % | dry | ISO 294-4 | Normal | ||
Density of melt | 1110 g/cm³ Show Supplier Material materials with Density of melt of 1110 g/cm³ | dry | - | ||
Specific heat capacity melt | 2830.0 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2830.0 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.28 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.28 W/(m·K) | dry | - | ||
Velocidad de flujo de la masa derretida | 24 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 24 g/10min | dry | ISO 1133 | ||
Velocidad de flujo del volumen derretido | 275 °C | 20 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 20 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Chainsaw housings, Powertool Housings, Skibinding Fixations, Inline Skate Frames, Airbag Containers | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |