General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 0.6 % Show Supplier Material materials with Absorción de agua of 0.6 % | dry | Sim. to ISO 62 |
Densidad | 0.77 g/cm³ Show Supplier Material materials with Densidad of 0.77 g/cm³ | dry | ISO 60 |
1.24 g/cm³ Show Supplier Material materials with Densidad of 1.24 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dureza Shore D | 58.0 [-] Show Supplier Material materials with Dureza Shore D of 58.0 [-] | dry | ISO 868 | 3s | |
Elongación | 50 % Show Supplier Material materials with Elongación of 50 % | dry | ISO 527-1/-2 | ||
300 % Show Supplier Material materials with Elongación of 300 % | dry | ISO 527-1/-2 | |||
Elongation at yield | 20 % Show Supplier Material materials with Elongation at yield of 20 % | dry | ISO 527-1/-2 | ||
Módulo elástico | 0.28 GPa Show Supplier Material materials with Módulo elástico of 0.28 GPa | dry | ISO 527-1/-2 | ||
Resistencia a desgarros | 152 kN/m Show Supplier Material materials with Resistencia a desgarros of 152 kN/m | dry | ISO 34-1; Method B | ||
Resistencia a la tracción | 36 MPa Show Supplier Material materials with Resistencia a la tracción of 36 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.85e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.85e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.85e-06 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.85e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 115 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 115 °C | dry | ISO 75-1/-2 | 0.45 MPa | |
Temperatura de fusión | 210 °C Show Supplier Material materials with Temperatura de fusión of 210 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de reblandecimiento Vicat | 125 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 125 °C | dry | ISO 306 | 50°C/h 50N | |
Temperatura de transición del vidrio | -60 °C Show Supplier Material materials with Temperatura de transición del vidrio of -60 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.4 [-] Show Supplier Material materials with Constante dieléctrica of 3.4 [-] | dry | IEC 62631-2-1 | 1MHz |
3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 110 [-] Show Supplier Material materials with Factor de disipación of 110 [-] | dry | IEC 62631-2-1 | 100Hz |
340 [-] Show Supplier Material materials with Factor de disipación of 340 [-] | dry | IEC 62631-2-1 | 1MHz | |
Rigidez dieléctrica | 22 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 22 kV/mm | dry | IEC 60243-1 | |
Volume resistivity | 1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 1.75 % Show Supplier Material materials with Contracción of 1.75 % | dry | Sim. to ISO 294-4 | Parallel | |
2 % Show Supplier Material materials with Contracción of 2 % | dry | Sim. to ISO 294-4 | Normal | ||
Velocidad de flujo del volumen derretido | 230 °C | 23 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 23 cm³/10min | dry | ISO 1133 |
Technological properties
Property |
---|