General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.04 % Show Supplier Material materials with Absorción de agua of 0.04 % | dry | ISO 62 | at 23°C after 24h |
Densidad | 1.86 g/cm³ Show Supplier Material materials with Densidad of 1.86 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 1.3 % Show Supplier Material materials with Elongación of 1.3 % | dry | ISO 527-1/-2 |
1.3 % Show Supplier Material materials with Elongación of 1.3 % | dry | ISO 527-1/-2 | ||
120 °C | 2.2 % Show Supplier Material materials with Elongación of 2.2 % | dry | ISO 527-1/-2 | |
160 °C | 2.3 % Show Supplier Material materials with Elongación of 2.3 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | |
120 °C | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | dry | ISO 178 | |
160 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
Módulo de flexión | 18 GPa Show Supplier Material materials with Módulo de flexión of 18 GPa | dry | ISO 178 | |
120 °C | 10 GPa Show Supplier Material materials with Módulo de flexión of 10 GPa | dry | ISO 178 | |
160 °C | 8 GPa Show Supplier Material materials with Módulo de flexión of 8 GPa | dry | ISO 178 | |
Módulo elástico | 19 GPa Show Supplier Material materials with Módulo elástico of 19 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | dry | ISO 527-1/-2 |
170 MPa Show Supplier Material materials with Resistencia a la tracción of 170 MPa | dry | ISO 527-1/-2 | ||
120 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | dry | ISO 527-1/-2 | |
160 °C | 75 MPa Show Supplier Material materials with Resistencia a la tracción of 75 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 9.8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9.8 kJ/m² | dry | ISO 179/1eA |
23 °C | 8.8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 8.8 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 40 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 40 kJ/m² | dry | ISO 179/1eU |
23 °C | 39 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 39 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.3e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.3e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | |
1.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
3.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
9e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 9e-07 1/K | dry | ISO 11359-1/-2 | normal, above Tg | ||
Temperatura de flexión bajo carga | 265 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 265 °C | dry | ISO 75-1/-2 | 2 MPa | |
Temperatura de fusión | 280 °C Show Supplier Material materials with Temperatura de fusión of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 90 °C Show Supplier Material materials with Temperatura de transición del vidrio of 90 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 [-] | dry | IEC 60250 | 5GHz |
Factor de disipación | 50 [-] Show Supplier Material materials with Factor de disipación of 50 [-] | dry | IEC 60250 | 5GHz |
Rigidez dieléctrica | 26 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 26 kV/mm | dry | IEC 60234 | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 175 V Show Supplier Material materials with Índice de seguimiento comparativo of 175 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Crankshaft Covers, Rectifier, Water pump part |