Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.16 g/cm³ Show Supplier Material materials with Densidad of 1.16 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.6 % Show Supplier Material materials with Moisture absorption of 2.6 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 4.8 % Show Supplier Material materials with Elongación of 4.8 % | dry | ISO 527-1/-2 | |
17 % Show Supplier Material materials with Elongación of 17 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 55.0 MPa Show Supplier Material materials with Flexural yield strength of 55.0 MPa | conditioned | ISO 178 | |
120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | ||
Módulo de flexión | 1.8 GPa Show Supplier Material materials with Módulo de flexión of 1.8 GPa | conditioned | ISO 178 | |
3.6 GPa Show Supplier Material materials with Módulo de flexión of 3.6 GPa | dry | ISO 178 | ||
Módulo elástico | 1.8 GPa Show Supplier Material materials with Módulo elástico of 1.8 GPa | conditioned | ISO 527-1/-2 | |
3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | 23 °C | 3 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 3 kJ/m² | dry | ISO 179/1eA |
23 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 6e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 6e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
7e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
Temperatura de flexión bajo carga | 70 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 70 °C | dry | ISO 75-1/-2 | 2 MPa | ||
192 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 192 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 100Hz |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 1MHz | |
Factor de disipación | 100 [-] Show Supplier Material materials with Factor de disipación of 100 [-] | dry | IEC 62631-2-1 | 100Hz |
200 [-] Show Supplier Material materials with Factor de disipación of 200 [-] | dry | IEC 62631-2-1 | 1MHz | |
Rigidez dieléctrica | 26 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 26 kV/mm | dry | IEC 60243-1 | |
Surface resistivity | 2e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 2e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 550 V Show Supplier Material materials with Índice de seguimiento comparativo of 550 V | dry | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Contracción | 1 % Show Supplier Material materials with Contracción of 1 % | dry | Sim. to ISO 294-4 | Parallel | |
1.1 % Show Supplier Material materials with Contracción of 1.1 % | dry | Sim. to ISO 294-4 | Normal | ||
Velocidad de flujo de la masa derretida | 230 °C | 40 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 40 g/10min | dry | ISO 1133 | |
Velocidad de flujo del volumen derretido | 230 °C | 39 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 39 cm³/10min | dry | ISO 1133 |