Ti6Al2Sn4Zr6Mo

Nombres alternativos y comerciales
Ti-Gr-6-2-4-6, Ti6-Al2-Sn4-Zr6-Mo, 6Al/2Sn/4Zr/6Mo, Alloy Titan 6AL-2Sn-4Zr-6Mo, Titanium 6-2-4-6
Want to keep this datasheet? Save it now in your required format

Description

Titanium 6-2-4-6 is a heat treatable alpha-beta alloy, with which you can achieve higher strengths than with Titanium 6/4. The advantages of Titanium 6-2-4-6 are an increased strength, low cycle fatigue and its ductility. It has a high strength at temperatures up to 450 ° C. Advantages of Titanium 6Al/2Sn/4Zr/6Mo


  • Low modulus of Elasticity
  • Low Density to Weight Ratio
  • Resistance to Fatigue
  • Heat Treatable to attain higher strengths

  • Equivalent Materials

    Los datos sobre este material han sido proporcionados por Hempel Special Metals.

    A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
    Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Propiedades

    General

    PropertyTemperatureValue

    Densidad

    23.0 °C

    4.5 g/cm³

    Show Supplier Material materials with Densidad of 4.5 g/cm³

    Mecánica

    PropertyTemperatureValueComment

    Módulo elástico

    23.0 °C

    70 GPa

    Show Supplier Material materials with Módulo elástico of 70 GPa

    114

    Aplicaciones térmicas

    PropertyTemperatureValue

    Calor específico

    23.0 °C

    420 J/(kg·K)

    Show Supplier Material materials with Calor específico of 420 J/(kg·K)

    Conductividad térmica

    23.0 °C

    22.6 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 22.6 W/(m·K)

    Temperatura de fusión

    1595 - 1675 °C

    Show Supplier Material materials with Temperatura de fusión of 1595 - 1675 °C

    Chemical properties

    PropertyValueComment

    Aluminio

    5.5 - 6.5 %

    Show Supplier Material materials with Aluminio of 5.5 - 6.5 %

    Carbono

    0.04 %

    Show Supplier Material materials with Carbono of 0.04 %

    max.

    Circonio

    3.6 - 4.4 %

    Show Supplier Material materials with Circonio of 3.6 - 4.4 %

    Cobre

    0.5 %

    Show Supplier Material materials with Cobre of 0.5 %

    max.

    Hidrógeno

    0.13 %

    Show Supplier Material materials with Hidrógeno of 0.13 %

    max.

    Hierro

    1.5 %

    Show Supplier Material materials with Hierro of 1.5 %

    max.

    Molibdeno

    5.5 - 6.5 %

    Show Supplier Material materials with Molibdeno of 5.5 - 6.5 %

    Nitrógeno

    0.04 %

    Show Supplier Material materials with Nitrógeno of 0.04 %

    max.

    Otro

    0.3 %

    Show Supplier Material materials with Otro of 0.3 %

    max.

    Oxígeno

    0.15 %

    Show Supplier Material materials with Oxígeno of 0.15 %

    max.

    Titanio

    Balance

    Technological properties

    Property
    Application areas

    Typical applications are in the intermediate stage compressors turbines, discs, blades and sour gas applications as well as in oil and gas industry.

    Other

    Beta Transus: 935°C

    The material is delivered with 3.1 certification. 3.2 Certification is available at extra cost.