General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 7.8 g/cm³ Show Supplier Material materials with Densidad of 7.8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Brinell | 23.0 °C | 270 [-] Show Supplier Material materials with Dureza Brinell of 270 [-] | max. |
Elongación A5 | 23.0 °C | 25 % Show Supplier Material materials with Elongación A5 of 25 % | min. |
Límite elástico Rp 0,2 | 23.0 °C | 500 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 500 MPa | min. |
Módulo elástico | 23.0 °C | 200 GPa Show Supplier Material materials with Módulo elástico of 200 GPa | |
Resistencia a la tracción | 23.0 °C | 700 - 900 MPa Show Supplier Material materials with Resistencia a la tracción of 700 - 900 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 23.0 °C | 500 J/(kg·K) Show Supplier Material materials with Calor específico of 500 J/(kg·K) |
Conductividad térmica | 23.0 °C | 15 W/(m·K) Show Supplier Material materials with Conductividad térmica of 15 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 8E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 8E-7 Ω·m |
Magnético
Property | Value |
---|---|
Magnetic properties | Magnetisation very low |
Chemical properties
Property | Value | Comment |
---|---|---|
Azufre | 0.015 % Show Supplier Material materials with Azufre of 0.015 % | max. |
Carbono | 0.03 % Show Supplier Material materials with Carbono of 0.03 % | max. |
Cobre | 1 - 2.5 % Show Supplier Material materials with Cobre of 1 - 2.5 % | |
Cromo | 24 - 26 % Show Supplier Material materials with Cromo of 24 - 26 % | |
Fósforo | 0.04 % Show Supplier Material materials with Fósforo of 0.04 % | max. |
Manganeso | 2 % Show Supplier Material materials with Manganeso of 2 % | max. |
Molibdeno | 3 - 4 % Show Supplier Material materials with Molibdeno of 3 - 4 % | |
Nitrógeno | 0.2 - 0.3 % Show Supplier Material materials with Nitrógeno of 0.2 - 0.3 % | |
Níquel | 6 - 8 % Show Supplier Material materials with Níquel of 6 - 8 % | |
Silicona | 0.7 % Show Supplier Material materials with Silicona of 0.7 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical & petrochemical, Ship building industry, Apparatus and tank construction, Turbine construction, Power plant construction, Transformer construction, Power engineering for onshore and offshore, Plant construction, Mechanical Engineering, Food industry | |
Corrosion properties | Very good corrosion and chemical resistance | |
General machinability | Good | |
Polishing ability | Good | |
Solution annealing | 1040-1120°C | |
Wear resistance | High resistance | |
Welding | TIG welding: limited, MAG Solid wire: limited, Arc welding: limited, UP welding: unsuitable, Laser beam welding: limited, Gas fusion welding: unsuitable | |
Workability | Hot forming: 1000-1200°C |