General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8 g/cm³ Show Supplier Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Brinell | 23.0 °C | 215 [-] Show Supplier Material materials with Dureza Brinell of 215 [-] | max. |
Elongación A5 | 23.0 °C | 28 % Show Supplier Material materials with Elongación A5 of 28 % | min. |
Límite elástico Rp 0,2 | 23.0 °C | 200 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 200 MPa | min. |
Módulo elástico | 23.0 °C | 200 GPa Show Supplier Material materials with Módulo elástico of 200 GPa | |
Resistencia a la tracción | 23.0 °C | 500 - 700 MPa Show Supplier Material materials with Resistencia a la tracción of 500 - 700 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 23.0 °C | 500 J/(kg·K) Show Supplier Material materials with Calor específico of 500 J/(kg·K) |
Conductividad térmica | 23.0 °C | 15 W/(m·K) Show Supplier Material materials with Conductividad térmica of 15 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 7.5E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 7.5E-7 Ω·m |
Magnético
Property | Value |
---|---|
Magnetic properties | Magnetisation is not possible |
Chemical properties
Property | Value | Comment |
---|---|---|
Azufre | 0.015 - 0.03 % Show Supplier Material materials with Azufre of 0.015 - 0.03 % | |
Carbono | 0.08 % Show Supplier Material materials with Carbono of 0.08 % | max. |
Cromo | 16.5 - 18.5 % Show Supplier Material materials with Cromo of 16.5 - 18.5 % | |
Fósforo | 0.04 % Show Supplier Material materials with Fósforo of 0.04 % | max. |
Manganeso | 2 % Show Supplier Material materials with Manganeso of 2 % | max. |
Molibdeno | 2 - 2.5 % Show Supplier Material materials with Molibdeno of 2 - 2.5 % | |
Níquel | 10.5 - 13.5 % Show Supplier Material materials with Níquel of 10.5 - 13.5 % | |
Silicona | 1 % Show Supplier Material materials with Silicona of 1 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | Apparatus engineering, Chemical industry, Textile Industry, Food Technology, Mechanical Engineering, Ship building, Medical technology & pharmacy | |
Corrosion properties | Very good | |
General machinability | Medium-not good | |
Solution annealing | 1020-1120°C | |
Welding | TIG welding: suitable, MAG Solid wire: suitable, Arc welding: suitable, UP welding: suitable, Laser beam welding: suitable, Gas fusion welding: suitable. It has a tendency to hot crack formation. | |
Workability | Hot forming: 900-1200°C |