General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 1.42 g/cm³ Show Supplier Material materials with Densidad of 1.42 g/cm³ | ASTM D792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 1 % Show Supplier Material materials with Elongación of 1 % | ASTM D638 |
Impact strength, Charpy notched, ASTM | 23.0 °C | 85 J/m Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 85 J/m | ASTM D256 |
Módulo de flexión | 23.0 °C | 15.9 GPa Show Supplier Material materials with Módulo de flexión of 15.9 GPa | ASTM D790 |
Resistencia a la flexión | 23.0 °C | 248 MPa Show Supplier Material materials with Resistencia a la flexión of 248 MPa | ASTM D790 |
Resistencia a la tracción | 23.0 °C | 214 MPa Show Supplier Material materials with Resistencia a la tracción of 214 MPa | ASTM D638 |
Aplicaciones térmicas
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 288 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 288 °C | ASTM D648 | |
Inflamabilidad | UL94 v0 |
Rheological Properties
Property | Temperature | Value |
---|---|---|
Contracción | 23.0 °C | 0.1 % Show Supplier Material materials with Contracción of 0.1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Aircraft parts, engine inner covers, bearings, gaskets, seals, clutch gear rings, valves and pumps, semiconductor industry, chemical industry, bars, surgical and dental equipment, military materials | |
Fillers | 30% Carbon Fiber |