General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.77 - 7.9 g/cm³ Show Material materials with Densidad of 7.77 - 7.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 24.0 °C | 0.23 - 0.24 [-] Show Material materials with Coeficiente de Poisson of 0.23 - 0.24 [-] |
149.0 °C | 0.27 - 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.27 - 0.31 [-] | |
260.0 °C | 0.26 - 0.35 [-] Show Material materials with Coeficiente de Poisson of 0.26 - 0.35 [-] | |
371.0 °C | 0.26 - 0.35 [-] Show Material materials with Coeficiente de Poisson of 0.26 - 0.35 [-] | |
483.0 °C | 0.29 - 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.29 - 0.3 [-] | |
593.0 °C | 0.26 - 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.26 - 0.29 [-] | |
704.0 °C | 0.29 - 0.36 [-] Show Material materials with Coeficiente de Poisson of 0.29 - 0.36 [-] | |
816.0 °C | 0.21 - 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.21 - 0.29 [-] | |
Dureza Brinell | 20.0 °C | 223 [-] Show Material materials with Dureza Brinell of 223 [-] |
Elongación | 20.0 °C | 30 % Show Material materials with Elongación of 30 % |
Elongación A80 | 20.0 °C | 28 % Show Material materials with Elongación A80 of 28 % |
Límite elástico Rp 0,2 | 20.0 °C | 230 MPa Show Material materials with Límite elástico Rp 0,2 of 230 MPa |
Límite elástico Rp 1,0 | 20.0 °C | 270 MPa Show Material materials with Límite elástico Rp 1,0 of 270 MPa |
Módulo de cizallamiento | 24.0 °C | 74.5 - 77.9 GPa Show Material materials with Módulo de cizallamiento of 74.5 - 77.9 GPa |
149.0 °C | 71 - 72.4 GPa Show Material materials with Módulo de cizallamiento of 71 - 72.4 GPa | |
260.0 °C | 66.2 - 69.6 GPa Show Material materials with Módulo de cizallamiento of 66.2 - 69.6 GPa | |
371.0 °C | 62.7 - 66.2 GPa Show Material materials with Módulo de cizallamiento of 62.7 - 66.2 GPa | |
483.0 °C | 61.4 - 62.1 GPa Show Material materials with Módulo de cizallamiento of 61.4 - 62.1 GPa | |
593.0 °C | 57.9 GPa Show Material materials with Módulo de cizallamiento of 57.9 GPa | |
704.0 °C | 52.4 - 53.8 GPa Show Material materials with Módulo de cizallamiento of 52.4 - 53.8 GPa | |
816.0 °C | 45.5 - 47.6 GPa Show Material materials with Módulo de cizallamiento of 45.5 - 47.6 GPa | |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 GPa Show Material materials with Módulo elástico of 196 GPa | |
24.0 °C | 193.7 GPa Show Material materials with Módulo elástico of 193.7 GPa | |
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
149.0 °C | 183.2 - 186.2 GPa Show Material materials with Módulo elástico of 183.2 - 186.2 GPa | |
200.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | |
260.0 °C | 175.1 - 178.6 GPa Show Material materials with Módulo elástico of 175.1 - 178.6 GPa | |
300.0 °C | 174 GPa Show Material materials with Módulo elástico of 174 GPa | |
371.0 °C | 166.2 - 169.6 GPa Show Material materials with Módulo elástico of 166.2 - 169.6 GPa | |
400.0 °C | 166 GPa Show Material materials with Módulo elástico of 166 GPa | |
483.0 °C | 159.3 - 160.7 GPa Show Material materials with Módulo elástico of 159.3 - 160.7 GPa | |
500.0 °C | 158 GPa Show Material materials with Módulo elástico of 158 GPa | |
593.0 °C | 146.2 - 148.9 GPa Show Material materials with Módulo elástico of 146.2 - 148.9 GPa | |
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
704.0 °C | 139.3 - 142 GPa Show Material materials with Módulo elástico of 139.3 - 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
816.0 °C | 110.3 - 122.7 GPa Show Material materials with Módulo elástico of 110.3 - 122.7 GPa | |
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | |
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | |
Resistencia a la tracción | 20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción of 550 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.84E-5 1/K | ||
600.0 °C | 1.8E-5 - 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.85E-5 - 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 - 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 1.95E-5 - 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.95E-5 - 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 12.6 - 15 W/(m·K) Show Material materials with Conductividad térmica of 12.6 - 15 W/(m·K) | |
100.0 °C | 14.1 W/(m·K) Show Material materials with Conductividad térmica of 14.1 W/(m·K) | ||
200.0 °C | 15.9 W/(m·K) Show Material materials with Conductividad térmica of 15.9 W/(m·K) | ||
300.0 °C | 17.4 W/(m·K) Show Material materials with Conductividad térmica of 17.4 W/(m·K) | ||
400.0 °C | 19 W/(m·K) Show Material materials with Conductividad térmica of 19 W/(m·K) | ||
500.0 °C | 20.5 - 21 W/(m·K) Show Material materials with Conductividad térmica of 20.5 - 21 W/(m·K) | ||
600.0 °C | 21.9 W/(m·K) Show Material materials with Conductividad térmica of 21.9 W/(m·K) | ||
700.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
800.0 °C | 24.7 W/(m·K) Show Material materials with Conductividad térmica of 24.7 W/(m·K) | ||
900.0 °C | 26.1 W/(m·K) Show Material materials with Conductividad térmica of 26.1 W/(m·K) | ||
1000.0 °C | 27.5 W/(m·K) Show Material materials with Conductividad térmica of 27.5 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.4 mm²/s Show Material materials with Difusividad térmica of 3.4 mm²/s | |
100.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | ||
200.0 °C | 3.9 mm²/s Show Material materials with Difusividad térmica of 3.9 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Difusividad térmica of 5.1 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
900.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
1000.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 1050 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 1050 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 8.5E-7 - 8.68E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 - 8.68E-7 Ω·m |
100.0 °C | 9.21E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.21E-7 Ω·m | |
200.0 °C | 9.75E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.75E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
600.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
700.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
800.0 °C | 1.21E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.21E-6 Ω·m | |
900.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
1000.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % |
Cromo | 19 - 21 % Show Material materials with Cromo of 19 - 21 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Nitrógeno | 0.11 % Show Material materials with Nitrógeno of 0.11 % |
Níquel | 11 - 13 % Show Material materials with Níquel of 11 - 13 % |
Silicona | 1.5 - 2.5 % Show Material materials with Silicona of 1.5 - 2.5 % |