General
Property | Value | Comment |
---|---|---|
Density | 2.65 - 2.7 g/cm³ Show Material materials with Density of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanical
Property | Value | Comment |
---|---|---|
Elastic modulus | 73.0 - 80.0 GPa Show Material materials with Elastic modulus of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium |
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100 °C | 0.0000209 1/K Show Material materials with Coefficient of thermal expansion of 0.0000209 1/K | nominal value between 20°C and the mentioned temperature |
300 °C | 0.0000229 1/K Show Material materials with Coefficient of thermal expansion of 0.0000229 1/K | nominal value between 20°C and the mentioned temperature | |
Melting point | 505.0 - 770.0 °C Show Material materials with Melting point of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | |
Specific heat capacity | 100 °C | 963 J/(kg·K) Show Material materials with Specific heat capacity of 963 J/(kg·K) | unstated value |
Thermal conductivity | 25 °C | 113 W/(m·K) Show Material materials with Thermal conductivity of 113 W/(m·K) | unstated value |