Kepstan® 6002

Alternative and trade names
PEKK
Want to keep this datasheet? Save it now in your required format

Description

KEPSTAN® PEKK resin is a high performance thermoplastic material, based on PolyEtherKetoneKetone (PEKK) highly stable chemical backbone. KEPSTAN® PEKK is a unique member of the PAEK family that incorporates distinctive structural features that allow for exceptional possibilities in the control of crystallinity. These features include a low Ether/Ketone ratio and a copolymer structure incorporating Terephtalic and Isophtalic moieties.

The 6000 Series represents the pseudo-amorphous products of the KEPSTAN® family, offering the lowest melting point and the slowest crystallization behavior, while keeping Tg close to 160°C. These properties allow for lower processing temperatures (as low as 320-330°C), and lead to glassy or semi crystalline structures, depending on processing technologies and cooling conditions.

KEPSTAN® 6000 Series includes a medium flow grade, KEPSTAN® 6002, and a high flow grade, KEPSTAN® 6003, both unfilled PEKK resins designed to meet the requirements of a broad range of processing technologies, including among others extrusion, calendering, thermoforming, injection molding, fiber impregnation, rotomolding, powder coating, bonding and welding.

KEPSTAN® PEKK resin is available in pellet form as well as in powder form with different particle sizes. Standard packaging includes 20 kg boxes for pellets and 10 kg boxes for powders.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Density

1.27 g/cm³

Show Supplier Material materials with Density of 1.27 g/cm³

dry

ISO 1183

Limiting oxygen index

38 %

Show Supplier Material materials with Limiting oxygen index of 38 %

dry

ISO 4589-1/-2

Mechanical

PropertyTemperatureValueConditionTesting Standard

Elastic modulus

2.9 GPa

Show Supplier Material materials with Elastic modulus of 2.9 GPa

dry

ISO 527-1/-2

Impact strength, Charpy notched

-30 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

dry

ISO 179/1eA

23 °C

5.5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5.5 kJ/m²

dry

ISO 179/1eA

Impact strength, Charpy unnotched

No Break at 23 and -30°C

dry

ISO 179/1eU

Thermal

PropertyValueConditionTesting StandardPressure

Heat deflection temperature

139 °C

Show Supplier Material materials with Heat deflection temperature of 139 °C

dry

ISO 75-1/-2

2 MPa

Electrical

PropertyValueConditionFrequencyTesting Standard

Dielectric constant

2.5 [-]

Show Supplier Material materials with Dielectric constant of 2.5 [-]

dry

1MHz

IEC 60250

Rheological Properties

PropertyValueConditionTesting StandardComment

Melt volume-flow rate

6 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 6 cm³/10min

dry

ISO 1133

380°C/1kg

Technological properties

Property
Application areas

Connectors,Fittings, Components, and Injection Molded Parts,Metal Tube Coating,Cable Ties,Chemical Process Industry,Chemical Process Industry - Coating of Chemical Pumps,Chemical Process Industry - Coating of Chemical Valves,Chemical Process Industry - Coating of Chemical Vessels,Chemical Process Industry - Injection Molding,Monofilaments,Packaging / Film,Powder Coatings - Wire Goods,Connectors E&E,Performance Wire,Wire and Cables,Natural Gas Distribution- Fittings

Processing methods

Injection Molding:

  • Drying temperature and time: 120°C for 6 to 8 hours
  • Processing temperature: 320 – 360°C
  • Temperature settings - Injection: Rear 300°C / Center 315°C / Front 320°C / Nozzle 330°C
  • Mold temperature (below Tg in any case): 80 - 120°C
  • Temperature settings - Extrusion Zones 1/2/3/4: 290°C/ 320°C/ 330°C/ 320°C Die: 320°C