Description

Kynar® resins are fluorinated thermoplastic homopolymers. Outstanding characteristics: chemical resistance, imperviousness to UV, high barrier properties, high purity, good mechanical and thermo-mechanical properties.

Kynar® 740 E resin is a standard grade of granules for extrusion of tubes and plaques, compression and transfer molding. This product is ANSI/NSF Standard 61 certified. This product is compliant with the EU positive list.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Density

1.78 g/cm³

Show Supplier Material materials with Density of 1.78 g/cm³

dry

ISO 1183

Limiting oxygen index

42 %

Show Supplier Material materials with Limiting oxygen index of 42 %

dry

ISO 4589-1/-2

Water absorption

0.008 %

Show Supplier Material materials with Water absorption of 0.008 %

Sim. to ISO 62

Mechanical

PropertyTemperatureValueConditionTesting StandardComment

Elastic modulus

2 GPa

Show Supplier Material materials with Elastic modulus of 2 GPa

dry

ISO 527-1/-2

Elongation

50 %

Show Supplier Material materials with Elongation of 50 %

dry

ISO 527-1/-2

min. | nominal

Elongation at yield

9 %

Show Supplier Material materials with Elongation at yield of 9 %

dry

ISO 527-1/-2

Impact strength, Charpy notched

23 °C

36 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 36 kJ/m²

dry

ISO 179/1eA

Yield strength

50 MPa

Show Supplier Material materials with Yield strength of 50 MPa

dry

ISO 527-1/-2

Thermal

PropertyValueConditionTesting StandardPressureComment

Coefficient of thermal expansion

0.00015 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.00015 1/K

dry

ISO 11359-1/-2

Glass transition temperature

-40 °C

Show Supplier Material materials with Glass transition temperature of -40 °C

dry

ISO 11357-1/-2

10°C/min

Heat deflection temperature

104 °C

Show Supplier Material materials with Heat deflection temperature of 104 °C

dry

ISO 75-1/-2

2 MPa

Melting point

169 °C

Show Supplier Material materials with Melting point of 169 °C

dry

ISO 11357-1/-3

10°C/min

Flammability

At thickness 1.6 mm IEC 60695-11-10: V-0 and yellow card available

Rheological Properties

PropertyValueConditionTesting StandardComment

Melt volume-flow rate

1.4 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 1.4 cm³/10min

dry

ISO 1133

230°C/3.8kg

Shrinkage

2.5 %

Show Supplier Material materials with Shrinkage of 2.5 %

dry

ISO 294-4

2.5 %

Show Supplier Material materials with Shrinkage of 2.5 %

dry

ISO 294-4

Transverse

Thermal conductivity of melt

0.19 W/(m·K)

Show Supplier Material materials with Thermal conductivity of melt of 0.19 W/(m·K)

Technological properties

Property
Application areas

Potable Water Distribution

Certifications

Yellow Card

Processing methods

Injection Molding:

  • Melt temperature (°C) ISO 294: 230
  • Mold temperature (°C) ISO 10724: 90
  • Injection velocity (mm/s) ISO 294: -
  • Pressure at hold (MPa) ISO 294: -