Description

Polyether block amide Pebax® 3533 SP 01 resin is a thermoplastic elastomer made of flexible polyether and rigid polyamide. This SP grade has been developed to be heat and UV resistant.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Abrasion resistance

64 mm³

Show Supplier Material materials with Abrasion resistance of 64 mm³

dry

ISO 4649

Density

1 g/cm³

Show Supplier Material materials with Density of 1 g/cm³

dry

ISO 1183

Moisture absorption

0.4 %

Show Supplier Material materials with Moisture absorption of 0.4 %

Sim. to ISO 62

Water absorption

1.2 %

Show Supplier Material materials with Water absorption of 1.2 %

Sim. to ISO 62

Mechanical

PropertyValueTesting StandardConditionComment

Compression set

22 [-]

Show Supplier Material materials with Compression set of 22 [-]

ISO 815

for 24h

Elastic modulus

0.018 GPa

Show Supplier Material materials with Elastic modulus of 0.018 GPa

ISO 527-1/-2

cond.

0.019 GPa

Show Supplier Material materials with Elastic modulus of 0.019 GPa

ISO 527-1/-2

dry

Elongation

50 %

Show Supplier Material materials with Elongation of 50 %

ISO 527-1/-2

cond., dry

min.

Hardness, Shore A

82 [-]

Show Supplier Material materials with Hardness, Shore A of 82 [-]

ISO 7619-1

for 3 seconds

Hardness, Shore D

25 [-]

Show Supplier Material materials with Hardness, Shore D of 25 [-]

ISO 7619-1

dry

15 seconds

Impact strength, Charpy notched

No Break at 23 and -30°C

ISO 179/1eA

cond.

Impact strength, Charpy unnotched

No Break at 23 and -30°C

ISO 179/1eU

cond.

Tear strength

50 kN/m

Show Supplier Material materials with Tear strength of 50 kN/m

ISO 34-1

Thermal

PropertyValueConditionTesting StandardComment

Coefficient of thermal expansion

0.00021 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.00021 1/K

dry

ISO 11359-1/-2

Glass transition temperature

-65 °C

Show Supplier Material materials with Glass transition temperature of -65 °C

dry

ISO 11357-1/-2

10°C/min

Melting point

144 °C

Show Supplier Material materials with Melting point of 144 °C

dry

ISO 11357-1/-3

10°C/min

Vicat softening temperature

77 °C

Show Supplier Material materials with Vicat softening temperature of 77 °C

ISO 306

50°C/h 50N

Flammability

At thickness 1.6 mm IEC 60695-11-10: HB and yellow card available

Electrical

PropertyValueConditionTesting StandardFrequency

Comparative tracking index

600 V

Show Supplier Material materials with Comparative tracking index of 600 V

cond.

IEC 60112

Dielectric constant

6 [-]

Show Supplier Material materials with Dielectric constant of 6 [-]

dry

IEC 60250

100Hz

6 [-]

Show Supplier Material materials with Dielectric constant of 6 [-]

dry

IEC 60250

1MHz

Dielectric strength

33.5 kV/mm

Show Supplier Material materials with Dielectric strength of 33.5 kV/mm

dry

IEC 60243-1

Dissipation factor

0.031 [-]

Show Supplier Material materials with Dissipation factor of 0.031 [-]

dry

IEC 60250

100Hz

0.0434 [-]

Show Supplier Material materials with Dissipation factor of 0.0434 [-]

dry

IEC 60250

1MHz

Surface resistivity

3e+12 Ω/sq

Show Supplier Material materials with Surface resistivity of 3e+12 Ω/sq

cond.

IEC 60093

Volume resistivity

3.2e+12 Ω·cm

Show Supplier Material materials with Volume resistivity of 3.2e+12 Ω·cm

dry

IEC 60093

Rheological Properties

PropertyValueConditionTesting StandardComment

Density of melt

0.83 g/cm³

Show Supplier Material materials with Density of melt of 0.83 g/cm³

Shrinkage

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

dry

ISO 294-4

0.8 %

Show Supplier Material materials with Shrinkage of 0.8 %

dry

ISO 294-4

Transverse

Specific heat capacity melt

2800 J/(kg·K)

Show Supplier Material materials with Specific heat capacity melt of 2800 J/(kg·K)

Thermal conductivity of melt

0.18 W/(m·K)

Show Supplier Material materials with Thermal conductivity of melt of 0.18 W/(m·K)

Technological properties

Property
Application areas

Fittings, Components, and Injection Molded Parts,Conveyor Belts and Pulleys,Footwear - Midsoles / Foam,Footwear - Outsoles,Sports Equipment

Certifications

Yellow Card

Processing methods

Injection Molding:

  • Typical melt temperature (Min / Recommended / Max) : 180°C / 210°C / 240°C.
  • Typical mold temperature : 10 – 30°C.
  • Drying time and temperature (only necessary for bags opened for more than two hours) : 4-8 hours at 55-65°C


    Extrusion:

  • Typical melt temperature (Min / Recommended / Max) : 190°C / 205°C / 220°C.