Pebax® 7033 SA 01

Alternative and trade names
TPA
Want to keep this datasheet? Save it now in your required format

Description

Polyether block amide Pebax® 7033 SA 01 resin is a thermoplastic elastomer made of flexible polyether and rigid polyamide. This SA grade is suitable for food contact applications.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Density

1.01 g/cm³

Show Supplier Material materials with Density of 1.01 g/cm³

dry

ISO 1183

Moisture absorption

1.1 %

Show Supplier Material materials with Moisture absorption of 1.1 %

Sim. to ISO 62

Water absorption

0.7 %

Show Supplier Material materials with Water absorption of 0.7 %

Sim. to ISO 62

Mechanical

PropertyTemperatureValueConditionTesting StandardComment

Elastic modulus

0.39 GPa

Show Supplier Material materials with Elastic modulus of 0.39 GPa

cond.

ISO 527-1/-2

0.414 GPa

Show Supplier Material materials with Elastic modulus of 0.414 GPa

dry

ISO 527-1/-2

Elongation

50 %

Show Supplier Material materials with Elongation of 50 %

cond., dry

ISO 527-1/-2

min. | nominal

Elongation at yield

20 %

Show Supplier Material materials with Elongation at yield of 20 %

cond.

ISO 527-1/-2

22 %

Show Supplier Material materials with Elongation at yield of 22 %

dry

ISO 527-1/-2

Hardness, Shore D

61 [-]

Show Supplier Material materials with Hardness, Shore D of 61 [-]

dry

ISO 7619-1

15 seconds

Impact strength, Charpy notched

-30 °C

20 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 20 kJ/m²

cond.

ISO 179/1eA

23 °C

120 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 120 kJ/m²

cond.

ISO 179/1eA

Impact strength, Charpy unnotched

No Break at 23 and -30°C

cond.

ISO 179/1eU

Yield strength

22 MPa

Show Supplier Material materials with Yield strength of 22 MPa

cond.

ISO 527-1/-2

23 MPa

Show Supplier Material materials with Yield strength of 23 MPa

dry

ISO 527-1/-2

Thermal

PropertyValueConditionTesting StandardComment

Melting point

172 °C

Show Supplier Material materials with Melting point of 172 °C

dry

ISO 11357-1/-3

10°C/min

Vicat softening temperature

164 °C

Show Supplier Material materials with Vicat softening temperature of 164 °C

ISO 306

50°C/h 50N

Rheological Properties

PropertyValueConditionTesting StandardComment

Shrinkage

1.2 %

Show Supplier Material materials with Shrinkage of 1.2 %

dry

ISO 294-4

1.5 %

Show Supplier Material materials with Shrinkage of 1.5 %

dry

ISO 294-4

Transverse

Technological properties

Property
Application areas

Main applications:

  • Athletic foot wear components
  • Food tubing
  • Note: this grade is not recommended by Arkema for usage in medical applications. For such applications Pebax® SA 01 MED should be used

    Packaging: This grade is delivered dried in sealed packaging (20 or 25 kg bags) ready to be processed.

    Shelf life: Two years from the delivery. For any use above this limit, please refer to our technical services.

  • Certifications

    Food Contact

    Processing methods

    Injection Molding:

  • Typical melt temperature (Min / Recommended / Max) : 230°C / 260°C / 290°C.
  • Typical mold temperature : 25 – 60°C.
  • Drying time and temperature (only necessary for bags opened for more than two hours) : 5-7 hours at 70-80°C.


    Extrusion:

  • Typical melt temperature (Min / Recommended / Max) : 220°C / 235°C / 250°C.
  • Drying time and temperature (only necessary for bags opened for more than two hours) : 5-7 hours at 70-80°C.