Rilsan® BMN BLACK TLD

Alternative and trade names
PA11
Want to keep this datasheet? Save it now in your required format

Description

PA11, MHLR, 12-010

Rilsan® BMN BLACK TLD resin is a polyamide 11 produced from a renewable source. This black grade is designed for injection molding. The percentage of renewable carbon according to ASTM D6866 (calculated) is 94%.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Bio-based content

94 %

Show Supplier Material materials with Bio-based content of 94 %

Density

1.03 g/cm³

Show Supplier Material materials with Density of 1.03 g/cm³

dry

ISO 1183

Limiting oxygen index

25 %

Show Supplier Material materials with Limiting oxygen index of 25 %

dry

ISO 4589-1/-2

Moisture absorption

0.8 %

Show Supplier Material materials with Moisture absorption of 0.8 %

Sim. to ISO 62

Water absorption

1.9 %

Show Supplier Material materials with Water absorption of 1.9 %

Sim. to ISO 62

Mechanical

PropertyTemperatureValueConditionTesting StandardComment

Elastic modulus

1.5 GPa

Show Supplier Material materials with Elastic modulus of 1.5 GPa

cond.

ISO 527-1/-2

Elongation

50 %

Show Supplier Material materials with Elongation of 50 %

cond.

ISO 527-1/-2

min. | nominal

Elongation at yield

6 %

Show Supplier Material materials with Elongation at yield of 6 %

cond.

ISO 527-1/-2

Hardness, Shore D

72 [-]

Show Supplier Material materials with Hardness, Shore D of 72 [-]

dry

ISO 7619-1

15 seconds

Impact strength, Charpy notched

-30 °C

7 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 7 kJ/m²

cond.

ISO 179/1eA

23 °C

6 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 6 kJ/m²

cond.

ISO 179/1eA

Impact strength, Charpy unnotched

No Break at 23 and -30°C

cond.

ISO 179/1eU

Yield strength

40 MPa

Show Supplier Material materials with Yield strength of 40 MPa

cond.

ISO 527-1/-2

Thermal

PropertyValueConditionTesting StandardComment

Coefficient of thermal expansion

8.5e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 8.5e-05 1/K

dry

ISO 11359-1/-2

Melting point

188 °C

Show Supplier Material materials with Melting point of 188 °C

dry

ISO 11357-1/-3

10°C/min

Vicat softening temperature

160 °C

Show Supplier Material materials with Vicat softening temperature of 160 °C

ISO 306

50°C/h 50N

Flammability

At thickness 3.2 IEC 60695-11-10: V-2 and yellow card available

Electrical

PropertyValueConditionTesting StandardFrequency

Comparative tracking index

600 V

Show Supplier Material materials with Comparative tracking index of 600 V

cond.

IEC 60112

Dielectric constant

3 [-]

Show Supplier Material materials with Dielectric constant of 3 [-]

dry

IEC 60250

1MHz

4 [-]

Show Supplier Material materials with Dielectric constant of 4 [-]

dry

IEC 60250

100Hz

Dielectric strength

30 kV/mm

Show Supplier Material materials with Dielectric strength of 30 kV/mm

cond.

IEC 60243-1

Dissipation factor

0.0262 [-]

Show Supplier Material materials with Dissipation factor of 0.0262 [-]

dry

IEC 60250

1MHz

0.0598 [-]

Show Supplier Material materials with Dissipation factor of 0.0598 [-]

dry

IEC 60250

100Hz

Surface resistivity

1e+14 Ω/sq

Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq

cond.

IEC 60093

Volume resistivity

1e+12 Ω·cm

Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm

cond.

IEC 60093

Rheological Properties

PropertyValueConditionTesting StandardComment

Melt volume-flow rate

36.5 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 36.5 cm³/10min

dry

ISO 1133

235°C/2.16kg

Shrinkage

0.4 %

Show Supplier Material materials with Shrinkage of 0.4 %

dry

ISO 294-4

0.8 %

Show Supplier Material materials with Shrinkage of 0.8 %

dry

ISO 294-4

Transverse

Technological properties

Property
Application areas

Main applications:

  • Injected parts

    Packaging: This grade is delivered dried in sealed packaging (25 kg bags) ready to be processed.

    Shelf life: Two years from the delivery. For any use above this limit, please refer to our technical services.

  • Certifications

    Yellow Card

    Processing methods

    Injection Molding:

  • Typical melt temperature (Min / Recommended / Max) : 210°C / 230°C / 280°C.
  • Mold temperature : 20 - 60°C
  • Drying time and temperature (only necessary for bags opened for more than two hours) : 4-6 hours at 80-90°C.