Rilsan® Clear G170

Alternative and trade names
PA*
Want to keep this datasheet? Save it now in your required format

Description

Rilsan® Clear G170 is a high performance transparent polyamide resin with outstanding thermal resistance. This grade has been designed for injection molding applications.

This material data has been provided by Arkema Technical Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Density

1.05 g/cm³

Show Supplier Material materials with Density of 1.05 g/cm³

dry

ISO 1183

Limiting oxygen index

26 %

Show Supplier Material materials with Limiting oxygen index of 26 %

dry

ISO 4589-1/-2

Moisture absorption

1.7 %

Show Supplier Material materials with Moisture absorption of 1.7 %

Sim. to ISO 62

Water absorption

3.8 %

Show Supplier Material materials with Water absorption of 3.8 %

Sim. to ISO 62

Mechanical

PropertyTemperatureValueConditionTesting StandardComment

Elastic modulus

2.0 GPa

Show Supplier Material materials with Elastic modulus of 2.0 GPa

cond.

ISO 527-1/-2

2.1 GPa

Show Supplier Material materials with Elastic modulus of 2.1 GPa

dry

ISO 527-1/-2

Elongation

50 %

Show Supplier Material materials with Elongation of 50 %

cond., dry

ISO 527-1/-2

min. | nominal

Elongation at yield

8 %

Show Supplier Material materials with Elongation at yield of 8 %

dry

ISO 527-1/-2

9 %

Show Supplier Material materials with Elongation at yield of 9 %

cond.

ISO 527-1/-2

Hardness, Shore D

79 [-]

Show Supplier Material materials with Hardness, Shore D of 79 [-]

dry

ISO 7619-1

15 seconds

Impact strength, Charpy notched

-30 °C

13 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m²

cond.

ISO 179/1eA

23 °C

13 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m²

cond.

ISO 179/1eA

Impact strength, Charpy unnotched

No Break at -30°C

dry and cond.

ISO 179/1eU

Yield strength

74 MPa

Show Supplier Material materials with Yield strength of 74 MPa

cond.

ISO 527-1/-2

Thermal

PropertyValueConditionTesting StandardComment

Coefficient of thermal expansion

7e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 7e-05 1/K

dry

ISO 11359-1/-2

Glass transition temperature

168 °C

Show Supplier Material materials with Glass transition temperature of 168 °C

dry

ISO 11357-1/-2

10°C/min

Vicat softening temperature

160 °C

Show Supplier Material materials with Vicat softening temperature of 160 °C

ISO 306

50°C/h 50N

Flammability

At thickness 1.6 mm IEC 60695-11-10: V-2 and yellow card available

Electrical

PropertyValueConditionTesting Standard

Comparative tracking index

600 V

Show Supplier Material materials with Comparative tracking index of 600 V

cond.

IEC 60112

Dielectric strength

50 kV/mm

Show Supplier Material materials with Dielectric strength of 50 kV/mm

cond.

IEC 60243-1

Surface resistivity

1e+12 Ω/sq

Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq

cond.

IEC 60093

Volume resistivity

1e+11 Ω·cm

Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm

cond.

IEC 60093

Optical

PropertyValueTesting Standard

Luminous transmittance

91 [-]

Show Supplier Material materials with Luminous transmittance of 91 [-]

ISO 13468-1/2

Rheological Properties

PropertyValueConditionTesting StandardComment

Melt volume-flow rate

2 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 2 cm³/10min

dry

ISO 1133

275°C/2.16kg

Shrinkage

0.7 %

Show Supplier Material materials with Shrinkage of 0.7 %

dry

ISO 294-4

0.7 %

Show Supplier Material materials with Shrinkage of 0.7 %

dry

ISO 294-4

Transverse

Technological properties

Property
Application areas

Home Appliance Tubing and Components

Certifications

Yellow Card

Processing methods

Injection Molding:

  • Typical melt temperature (Min / Recommaneded / Max) : 270°C / 290°C / 310°C
  • Typical mold temperature : 40 - 80 °C
  • Dyring time and temperature (only for bags opened for more than two hours): 4 - 6 hours at 90°C


    Film Extrusion:

  • Typical melt temperature (Min / Recommaneded / Max) : 270°C / 280°C / 290°C
  • Dyring time and temperature (only for bags opened for more than two hours): 4 - 6 hours at 90°C