PA11, M, 18-010

Rilsan® KNO resin is a polyamide 11 resin produced from a renewable source. This natural grade is specially designed for injection molding. The percentage of renewable carbon according to ASTM D6866 (calculated) is 100%.

This material data has been provided by Arkema High Performance Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Bio-based content

100 %

Show Supplier Material materials with Bio-based content of 100 %

ASTM D6866

Density

23.0 °C

1.03 g/cm³

Show Supplier Material materials with Density of 1.03 g/cm³

ISO 1183

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

1.25 GPa

Show Supplier Material materials with Elastic modulus of 1.25 GPa

ISO 527-1/-2

Elongation

23.0 °C

50 %

Show Supplier Material materials with Elongation of 50 %

min., ISO 527-1/-2, nominal

Elongation at yield

23.0 °C

4 %

Show Supplier Material materials with Elongation at yield of 4 %

ISO 527-1/-2

Hardness, Shore D

23.0 °C

73 [-]

Show Supplier Material materials with Hardness, Shore D of 73 [-]

ISO 7619-1, 15 seconds

Impact strength, Charpy notched

-30.0 °C

13 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m²

23.0 °C

11 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 11 kJ/m²

Yield strength

23.0 °C

37 MPa

Show Supplier Material materials with Yield strength of 37 MPa

ISO 527-1/-2

Impact strength, Charpy unnotched

No break @ 23,-30°C, ISO 179/1eU

Thermal

PropertyValueComment

Melting point

189 °C

Show Supplier Material materials with Melting point of 189 °C

ISO 11357-1/-3, 10°C/min

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.7 %

Show Supplier Material materials with Shrinkage of 0.7 %

ISO 294-4 2577

Shrinkage, transverse

23.0 °C

0.7 %

Show Supplier Material materials with Shrinkage, transverse of 0.7 %

ISO 294-4 2577

Technological properties

Property
Application areas

Main applications:

  • Injected parts

  • Other

    Packaging:

  • This grade is delivered dried in sealed packaging (25 kg bags) ready to be processed.

    Shelf Life:

  • Two years from the delivery. For any use above this limit, please refer to our technical services.

  • Processing methods

    Injection Molding:

  • Typical melt temperature (Min / Recommended / Max) : 230°C / 250°C / 270°C.
  • Mold temperature : 20 - 40°C
  • Drying time and temperature (only necessary for bags opened for more than two hours) : 4-6 hours at 80-90°C.