Rilsan® TIEFLEX S442 NAT TL

Alternative and trade names
PA*
Want to keep this datasheet? Save it now in your required format

Description

Rilsan ® TIEFLEX S442 NAT TL resin is a flexible tie layer alloy partially based on renewable resources. This grade is designed for multilayer automotive and trucks fuel lines (tie layer for fuel line).

This material data has been provided by Arkema High Performance Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.06 g/cm³

Show Supplier Material materials with Density of 1.06 g/cm³

ISO 1183

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

50 %

Show Supplier Material materials with Elongation of 50 %

min., ISO 527-1/-2, nominal, Conditioned

Elongation at yield

23.0 °C

40 %

Show Supplier Material materials with Elongation at yield of 40 %

ISO 527-1/-2, Conditioned

Yield strength

23.0 °C

31 MPa

Show Supplier Material materials with Yield strength of 31 MPa

ISO 527-1/-2, Conditioned

Thermal

PropertyValueComment

Melting point

217 °C

Show Supplier Material materials with Melting point of 217 °C

ISO 11357-1/-3, 10°C/min

Rheological Properties

PropertyValueComment

Melt volume-flow rate

4.6 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 4.6 cm³/10min

ISO 1133, 235°C/5kg

Technological properties

Property
Application areas

Fuel Management - Fuel Lines

Other

Packaging:

This grade is delivered dried in sealed packaging (25kg bags) ready to be processed.

Shelf life:

Two years from the date of delivery. For any use above this limit, please refer to our technical services.

Processing methods

Extrusion:

  • Typical melt temperature (min / recommended / max): 220°C / 230°C / 240°C
  • Drying time and temperature (only necessary for bags opened for more than two hours): 4-6 hours at 80°C