Description

Carbon - Chopped Fibre - C 006560 is a high strength, PAN based fiber

Related Standards

Ashby charts

See where falls on the material property chart for Density against Elastic modulus in your materials selection and design process.

Properties

General

Density ρ

1.8 g/cm³ at 20 °C

SRM 15 (typical fibre properties)

Yield 12K Y12K

800 mg/m at 20 °C

SRM 13

Yield 24K Y24K

1600 mg/m at 20 °C

SRM 13

Dimension

Diameter d

6.999999999999999E-3 mm

Length l

6 mm

fiber length

Mechanical

Compressive modulus Ecomp

127 MPa at 20 °C

ASTM D3039

Compressive modulus, transverse Ecomp,trans

10.2 MPa at 20 °C

ASTM D3039

Compressive strength Rmc

1365 MPa at 20 °C

ASTM D3039

Compressive strength, transverse Rs,trans

196 MPa at 20 °C

ASTM D3039

Elastic modulus E

137 GPa at 20 °C

ASTM D3039

Elastic modulus, transverse E

9.2 GPa at 20 °C

ASTM D3039

Flexural modulus Ebend

132 GPa at 20 °C

ASTM D790 (L/D=32, Vf=61%)

Flexural modulus, transverse Ebend,trans

8.8 GPa at 20 °C

ASTM D790 (L/D=32, Vf=61%)

Flexural strength σbend

1745 MPa at 20 °C

ASTM D790 (L/D=32, Vf=61%)

Flexural strength, transverse σbendT

102 MPa at 20 °C

ASTM D790 (L/D=32, Vf=61%)

Interlaminar shear strength ILSS

97 MPa at 20 °C

ASTM D2344 (L/D=4, Vf=59%)

Tensile strength Rm

2572 MPa at 20 °C

ASTM D3039

Tensile strength, transverse Rm,trans

81 MPa at 20 °C

ASTM D3039

Tow tensile modulus Etow

234 GPa at 20 °C

SRM 16 (typical fibre properties)

Tow tensile strength Rm,two

4830 MPa at 20 °C

SRM 16 (typical fibre properties)

Technological properties

Processing history

Epoxy sized 1.2%

This material data has been provided by Goodfellow.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.