BrushForm® 158 Strip TM04 (C72900)

Alternative and trade names
BrushForm® 158 Strip Mill Hardened Tempers
Want to keep this datasheet? Save it now in your required format

Description

Materion Brush Performance Alloys’ BrushForm® 158 Strip is a high-performance, heat treatable spinodal copper nickel tin alloy designed to provide optimal formability and strength characteristics in conductive spring applications such as electronic connectors, switches, and sensors. The higher strength tempers provide excellent fatigue and impact performance making them ideal for voice coil motor springs in optical image stabilization systems. BrushForm 158 strip is available in both pre-heat treated (mill hardened) and heat treatable (age hardenable) forms.

Related Standards

This material data has been provided by Materion Brush GmbH.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

9 g/cm³

Show Supplier Material materials with Density of 9 g/cm³

Dimension

PropertyValueComment

Thickness

0.04 - 0.5 mm

Show Supplier Material materials with Thickness of 0.04 - 0.5 mm

gauge

Mechanical

PropertyTemperatureValueComment

Bendability 90°, bw

23.0 °C

1 [-]

Show Supplier Material materials with Bendability 90°, bw of 1 [-]

Bendability 90°, gw

23.0 °C

1 [-]

Show Supplier Material materials with Bendability 90°, gw of 1 [-]

Elastic modulus

23.0 °C

128 GPa

Show Supplier Material materials with Elastic modulus of 128 GPa

Elongation

23.0 °C

10 %

Show Supplier Material materials with Elongation of 10 %

for strip thicker than 0.10 mm

Hardness, Vickers

23.0 °C

245 - 345 [-]

Show Supplier Material materials with Hardness, Vickers of 245 - 345 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Supplier Material materials with Poisson's ratio of 0.3 [-]

Tensile strength

23.0 °C

895 MPa

Show Supplier Material materials with Tensile strength of 895 MPa

Yield strength Rp0.2

23.0 °C

790 - 900 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 790 - 900 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.64E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.64E-5 1/K

Electrical

PropertyTemperatureValue

Electrical conductivity

23.0 °C

4.00E+6 S/m

Show Supplier Material materials with Electrical conductivity of 4.00E+6 S/m

Specific Electrical conductivity

7 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 7 % IACS

Magnetic

PropertyTemperatureValue

Relative magnetic permeability

23.0 °C

1.01 [-]

Show Supplier Material materials with Relative magnetic permeability of 1.01 [-]

Chemical properties

PropertyValue

Copper

Balance

Nickel

14.5 - 15.5 %

Show Supplier Material materials with Nickel of 14.5 - 15.5 %

Tin

7.5 - 8.5 %

Show Supplier Material materials with Tin of 7.5 - 8.5 %

Technological properties

Property
Application areas

Voice coil motor springs (VCM), Optical image stabilization systems (OIS) & Electromagnetic shielding gaskets.