Description

Materion Performance Alloys’ nickel beryllium strip Alloy 360 (UNS number N03360) combines unique mechanical and physical properties.


Properties of nickel beryllium Alloy 360 strip that a designer can use include ultimate tensile strength approaching 300,000 psi (2000 MPa), yield strength up to 245,000 psi (1690 MPa), excellent formability, stress relaxation less than 5% at 400º F (200°C), and fatigue strength (in reverse bending) of 85,000-90,000 psi (586-655 MPa) at 10 million cycles. It has corrosion resistance surpassing stainless steel. Typically, this alloy is used for mechanical and electrical / electronic components that are subjected to elevated temperatures (up to 700º F / 370°C for short times), and require good spring characteristics at these temperatures.

This material data has been provided by Materion Brush GmbH.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.27 g/cm³

Show Supplier Material materials with Density of 8.27 g/cm³

Mechanical

PropertyTemperatureValueComment

Bendability 90°, bw

23.0 °C

0 [-]

Show Supplier Material materials with Bendability 90°, bw of 0 [-]

Bendability 90°, gw

23.0 °C

0 [-]

Show Supplier Material materials with Bendability 90°, gw of 0 [-]

Elastic modulus

23.0 °C

195 - 210 GPa

Show Supplier Material materials with Elastic modulus of 195 - 210 GPa

Elongation

23.0 °C

30 %

Show Supplier Material materials with Elongation of 30 %

min., for strip thicker than 0.10 mm

Hardness, Rockwell A

23.0 °C

39 - 57 [-]

Show Supplier Material materials with Hardness, Rockwell A of 39 - 57 [-]

Hardness, Vickers

23.0 °C

106 - 200 [-]

Show Supplier Material materials with Hardness, Vickers of 106 - 200 [-]

Tensile strength

23.0 °C

660 - 900 MPa

Show Supplier Material materials with Tensile strength of 660 - 900 MPa

Yield strength Rp0.2

23.0 °C

280 - 480 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 280 - 480 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.45E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.45E-5 1/K

Melting point

1195 - 1325 °C

Show Supplier Material materials with Melting point of 1195 - 1325 °C

Thermal conductivity

23.0 °C

48 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 48 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

4.31E-7 Ω·m

Show Supplier Material materials with Electrical resistivity of 4.31E-7 Ω·m

Specific Electrical conductivity

4 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 4 % IACS

Chemical properties

PropertyValueComment

Beryllium

1.85 - 2.05 %

Show Supplier Material materials with Beryllium of 1.85 - 2.05 %

Copper

0.25 %

Show Supplier Material materials with Copper of 0.25 %

max.

Nickel

Balance

Technological properties

Property
Application areas

Some applications for this alloy are Belleville washers for fire protection sprinkler heads, thermostats, bellows, diaphragms, connectors and burn-in and test sockets electrical /electronic systems.

Plating

Alloy 360 strip when properly cleaned exhibits surface chemistry characteristics similar to other commercial nickel base alloys. Techniques and procedures for plating and joining commercial nickel base alloys can be used on nickel beryllium.

Workability

Excellent - Used for deep-drawn and severely cupped or formed parts; can be bent flat through 180° angle in any direction